Next Article in Journal
Converging Artificial Intelligence and Quantum Technologies: Accelerated Growth Effects in Technological Evolution
Next Article in Special Issue
Effect of Oscillating Area on Generating Microbubbles from Hollow Ultrasonic Horn
Previous Article in Journal
Atomic Quantum Technologies for Quantum Matter and Fundamental Physics Applications
Previous Article in Special Issue
Hunting Search Algorithm-Based Adaptive Fuzzy Tracking Controller for an Aero-Pendulum
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Fluorine-Free Single-Component Polyelectrolyte of Poly(ethylene glycol) Bearing Lithium Methanesulfonylsulfonimide Terminal Groups: Effect of Structural Variance on Ionic Conductivity

Graduate School of Science and Engineering, Yamagata University, Yonezawa 990-8510, Japan
*
Author to whom correspondence should be addressed.
Current Address: Department of Applied Chemistry, Faculty of Engineering, Osaka Institute of Technology, Osaka 535-8585, Japan.
Technologies 2024, 12(5), 65; https://doi.org/10.3390/technologies12050065
Submission received: 9 April 2024 / Revised: 30 April 2024 / Accepted: 7 May 2024 / Published: 9 May 2024
(This article belongs to the Special Issue Smart Systems (SmaSys2023))

Abstract

:
Fluorine-free single-component polyelectrolytes were developed via the hybridization of lithium methanesulfonylsulfonimide (LiMSSI) moieties to poly(ethylene glycol) (PEG) derivatives with different morphologies, and the relationship between the structure and its ionic conductivity was investigated. The PEG-LiMSSI derivatives with one, two, and three LiMSSI end groups were prepared via the concomitant Michael-type addition and lithiation of PEGs and N-methanesulfonylvinylsulfonimide. The ionic conductivity at 60 °C ranged from 1.8 × 10−7 to 2.0 × 10−4 S/cm. PEG-LiMSSI derivatives with one LiMSSI terminus and with two LiMSSI termini at both ends show higher ionic conductivity, that is as good as fluorine-free single-component polyelectrolytes, than that with two LiMSSI termini at one end and that with three LiMSSI termini.

1. Introduction

Lithium-ion batteries are used in a wide range of applications, from large batteries for automobiles and smart grids to small batteries for mobile devices. In recent years, polymer-type batteries, which have a lower risk of leakage and thus allow for simpler packaging, have become more widespread [1,2,3,4]. Their disadvantage is their low ionic conductivity. In addition, typical gel electrolytes, consisting of polymers and low-molecular-weight lithium salts, suffer from the predominant transference of anions over lithium cations because lithium cations are ligated by polymers such as poly(ethylene glycol) (PEG) to reduce their relative mobility. To overcome this problem, polymers with immobilized anion structures in their backbones have been designed to suppress the migration of anions. Carboxylates, sulfonates, sulfonamides, and trifluoromethanesulfonylsulfonimides are typical anionic structures for linking to organic backbones, and various single-component polyelectrolytes without low-molecular-weight anions have been developed.
Anions hybridized with PEG for conducting lithium cations are typical examples. Ohno et al. developed a series of single-component electrolytes of PEG derivatives with carboxylate [5], sulfonate [6,7], and sulfonamide [8,9] termini with ionic conductivities of 10−6–10−7 S/cm at ambient temperatures. The migration of anions is successfully suppressed by reducing the mobility of anions, but the total ionic conductivities are insufficient. Various researchers have developed PEG derivatives with other anions to improve ionic conductivity. Aluminates consisting of PEG chains and fluorinated anions developed by Fujinami et al. show ionic conductivities of 10−5 S/cm at room temperature [10]. Subsequently, borate analogs were developed and showed similar ionic conductivities [11,12,13,14]. Despite the improved ionic conductivity, the low stabilities of aluminum and boron alkoxides are problematic. The introduction of one alkyl chain, one fluorinated alkoxy group, and two tri(ethylene glycol) chains on boron resulted in higher stability and ion conductivity (>10−4 S/cm−1 at room temperature) [15]. PEGs with bis(fluoroalkanesulfonyl)imide ends [16,17] and a 1,2,3-triazolate [18] end were also designed and exhibited ionic conductivities of 10−6 and 10−7 S/cm at room temperature, respectively. Block copolymers composed of PEG chains and styrene-based fluorinated polyanions [19,20,21] and cross-linked PEG derivatives with lithium sulfonate and trifluoromethanesulfonylsulfonimide ends [22] have also been developed.
Most polymers with higher ionic conductivity contain fluorinated structures to stabilize anions, as described later. However, the fluorinated organic groups increase the environmental risk [23,24] and the price. Accordingly, both low-molecular-weight and polymeric fluorine-free electrolytes are in high demand [25,26,27,28,29,30,31]. For the stable hybridization of fluorine-free organic structures and anions, we focused on bis(alkanesulfonyl)imide moieties that carry the anion on the nitrogen atom delocalized by two sulfonimide groups with strong electron-withdrawing properties. Lithium bis(alkanesulfonyl)imide derivatives have good ionic conductivities despite their low solubilities [25].
We applied the lithium methanesulfonylsulfonimide (LiMSSI) moieties to polymers with copolymers of PEG methacrylate (PEGMA) and lithium-N-methanesulfonylvinylsulfonimide (LiMSVSI), a vinyl monomer with a similar structure to lithium trifluoromethanesulfonimide (LiTFSI), which exhibit good ionic conductivities of 8.4 × 10−5 and 9.2 × 10−4 S/cm at 25 and 90 °C, respectively [31]. The problem of the poor solubility was overcome by copolymerization. However, LiMSVSI has a low radical polymerizability, which limits the density of the lithium salt structure lower.
During the synthesis of LiMSVSI, we found that ethanol nucleophilically adds to the vinyl group of N-methanesulfonylvinylsulfonimide (MSVSI) via the Michael-type addition with the simultaneous lithiation of the sulfonimide group. We extended this finding to the design of PEGs bearing LiMSSI terminal groups without additional salts and solvents. Furthermore, different derivatives were synthesized and evaluated to investigate the effects of factors on the ionic conductivities. The LiMSSI-terminated PEG derivatives examined are PEGs with one, two, and three terminal LiMSSI groups with different molecular weights (Figure 1). In this study, we clarified the effect of the structural variance, namely, how the molecular weight of the PEG segment, the modification ratio of terminal LiMSSI, the number of terminal LiMSSI groups, and the morphological arrangement of terminal LiMSSI groups affect the ionic conduction behavior and the glass transition temperature (Tg), a controlling factor for ionic conductivity, of PEGs with terminal LiMSSI structures.

2. Materials and Methods

2.1. Materials

All the reagents were used as received. MSVSI [30] and 3-[2-(2-methoxyethoxy)ethoxy]-1,2-propanediol (DMEMME diol) [32] were prepared as reported. LiOH monohydrate, tetrahydrofuran (THF), methanol, acetone, ethyl acetate, methylene dichloride, PEG with an Mn of 1000 (PEG1000), and diethyl carbonate (DEC) were purchased from Kanto Chemical (Tokyo, Japan). PEG monomethyl ether with a number-average molecular weight (Mn) of 400 (PEG400MME), PEG monomethyl ether with an Mn of 1000 (PEG1000MME), PEG with an Mn of 200 (PEG200), PEG with an Mn of 400 (PEG400), and LiTFSI were purchased from Tokyo Chemical Industry (Tokyo, Japan). Trimethylolpropane ethoxylate (Mn = ca. 450) (TMPE450) was purchased from Sigma-Aldrich (St. Louise, MO, USA). Ethylene carbonate (EC) was purchased from Wako Pure Chemical (Osaka, Japan).

2.2. Measurements

2.2.1. Instruments

1H NMR spectra were measured on a JEOL (Tokyo, Japan) ECX-400 spectrometer using D2O as the solvent (23–25 °C, relaxation delay = 5 s, 8 scans). The residual solvent signal of DHO was used as the internal reference. 7Li NMR spectra were measured on a JEOL (Tokyo, Japan) ECX-500 spectrometer using D2O as the solvent (23–25 °C, relaxation delay = 2 s, 24 scans). Differential scanning calorimetry (DSC) measurements were performed on a Seiko (Tokyo, Japan) DSC-220 instrument under a nitrogen atmosphere (10 °C/min, N2, with a second heating scan after heating to 100 °C and cooling to −80 °C at 10 °C/min). Cyclic voltammetric (CV) analyses were carried out on a CH Instruments (Austin, TX, USA) CHI704E potentiostat at the scan rate of 0.1 V/s. All the measurements were performed in a 1.0 M LiTFSI solution of EC/DEC (v/v = 3/7) at ambient temperature using a three-electrode system, with each solution being purged with nitrogen prior to measurement. The working electrode was a Pt disk (ϕ = 5 mm, BAS, Tokyo, Japan), the counter electrode was a Pt wire (ϕ = 0.5 mm, BAS, Tokyo, Japan), and the reference electrode was an Ag wire (ϕ = 1 mm, Nilaco, Tokyo, Japan).

2.2.2. Measurement of Ion Conductivity

Ionic conductivities were measured using a Hioki (Nagano, Japan) 3532-80 electrochemical impedance spectrometer. A two-point-probe conductivity cell with two platinum plate electrodes was fabricated. The cell was placed in a nitrogen-filled plastic bag in an EYELA (Tokyo, Japan) VOS-300VD thermo-controlled chamber. The samples were dried at 90 °C under a vacuum for at least 10 h prior to the measurement and were treated under a nitrogen atmosphere. The chamber temperature was raised to approximately 100 °C, and the temperature around the samples was measured using a digital thermometer placed aside from the samples. The samples were annealed for 1 h, and the chamber temperature was lowered. Ionic conductivity was monitored as a gradual decrease in the temperature of the samples. Ionic conductivity (σ) was calculated from following Equation (1).
σ = d/(L W R)
In the equation, d, L, W, and R are the distance between the two electrodes (cm), the length of electrode (cm), the width of electrode (cm), and the resistance value (Ω), respectively.

2.3. Synthesis of Polymers

2.3.1. Synthesis of DEGMME-LiMSSI2

DEGMME diol (58.8 mg, 300 μmol), MSVSI (111 mg, 600 μmol), and lithium hydroxide monohydrate (50.4 mg, 600 μmol) were added to a 20 mL round-bottom flask. Then, the flask was degassed and purged with nitrogen. The mixture was magnetically stirred in an oil bath maintained at 100 °C for 48 h. The resulting viscous material was dissolved in THF, and the soluble portion was collected via filtration. The solvent was removed using an evaporator, and MSVSI (93–185 mg, 0.50–1.00 mmol) was added again and stirred at 100 °C for 48 h. This procedure was repeated two or three times until the introduction efficiency of the LiMSSI group became constant.
For purification, THF was first added. The soluble portion was collected to remove LiOH, and THF was evaporated off under a vacuum. Next, the product was re-precipitated using 15 mL of THF as a good solvent and 300 mL of ethyl acetate as a poor solvent. The resulting dispersion was centrifuged, and the supernatant was removed. The precipitate was collected via dissolving in methanol to give a DEGMME derivative with two LiMSSI termini (DEGMME-LiMSSI2) (yield = 20 mg and 12%, introduction ratio of LiMSSI termini 89%).
1H-NMR (400 MHz, D2O, δ in ppm): 3.38 (s, 3H, –SO2CH3), 3.43 (t, J = 6.2 Hz, 2H, >CHOCH2CH2SO2–), 3.50 (t, J = 6.2 Hz, 2H, –CH2OCH2CH2SO2–), 3.50–3.80 (br, polyether backbone), 3.96 (t, J = 5.5 Hz, 2H, –CH2OCH2CH2SO2–), 4.00 (t, J = 5.5 Hz, 2H, >CH2OCH2CH2SO2–).
7Li-NMR (194 MHz, D2O, δ in ppm): 2.96 (N–Li).

2.3.2. Synthesis of TMPE450-LiMSSI3

TPME450 (900 mg, 2.00 mmol), MSVSI (1.11 g, 6.00 mmol), and lithium hydroxide monohydrate (378 mg, 9.00 mmol) were added to a 20 mL round-bottom flask. Then, the flask was degassed and purged with nitrogen. The mixture was magnetically stirred in an oil bath maintained at 100 °C for 48 h. The resulting viscous material was dissolved in THF, and the soluble portion was collected via filtration. The solvent was removed using an evaporator, and MSVSI (93–185 mg, 0.50–1.00 mmol) was added again and stirred at 100 °C for 48 h. This procedure was repeated two or three times until the quantitative introduction of the LiMSSI group.
For purification, acetone was first added, and the mixture was sonicated for 1 h. The soluble portion was collected to remove LiOH, and acetone was evaporated off under a vacuum. Next, the product was re-precipitated using 15 mL of acetone as a good solvent and 300 mL of methylene dichloride as a poor solvent. The resulting dispersion was centrifuged, and the supernatant was removed. The precipitate was collected via dissolving in methanol to give a TPME450 derivative with three LiMSSI termini (TPME450-LiMSSI3) (yield = 530 mg and 25%, introduction ratio of LiMSSI termini > 86%).
1H-NMR (400 MHz, D2O, δ in ppm): 0.85 (t, J = 7.5 Hz, 3H, –CH2CH3), 1.35 (q, J = 7.5 Hz, 2H, –CH2CH3), 3.08 (s, 3H, –SO2CH3), 3.42 (s, EtC(CH2O)3–), 3.49 (t, J = 6.4 Hz, 2H, –CH2CH2SO2–), 3.63–3.75 (4nH, –OCH2CH2O–), 3.93 (t, J = 6.3 Hz, 2H, –CH2CH2SO2–).
7Li-NMR (194 MHz, D2O, δ in ppm): 2.96 (N–Li).

2.3.3. Synthesis of PEG200-LiMSSI2 (Typical Procedure)

PEG with an Mn of 200 (PEG200) (2.00 g, 10.0 mmol), MSVSI (3.70 g, 20.0 mmol), and lithium hydroxide monohydrate (1.68 g, 40.0 mmol) were added to a 20 mL round-bottom flask. Then, the flask was degassed and purged with nitrogen. The mixture was magnetically stirred in an oil bath maintained at 100 °C for 48 h. The resulting viscous material was dissolved in methylene dichloride, and the soluble portion was collected via filtration. The solvent was removed using an evaporator, and MSVSI (93–185 mg, 0.50–1.00 mmol) was added again and stirred at 100 °C for 48 h. This procedure was repeated two or three times.
For purification, methylene chloride was first added to the product and sonicated for 1 h. The soluble portion was collected, and methylene dichloride was removed under a vacuum. Next, the product was re-precipitated using 15 mL of ethanol as a good solvent and 300 mL of ethyl acetate as a poor solvent. The resulting dispersion was centrifuged, and the supernatant was removed. The precipitate was collected via dissolving in methanol to give a PEG200 derivative with two LiMSSI termini (PEG200-LiMSSI2) (yield = 0.84 g and 34%, introduction ratio of LiMSSI termini > 99%).
1H-NMR (400 MHz, D2O, δ in ppm): 3.01 (s, 3H, –SO2CH3), 3.53 (t, J = 6.4 Hz, 2H, –CH2CH2SO2–), 3.59–3.69 (-4nH, –OCH2CH2O–), 3.88 (t, J = 6.4 Hz, 2H, –CH2SO2–).
7Li-NMR (194 MHz, D2O, δ in ppm): 2.96 (N–Li).

2.3.4. Synthesis of Other Polymers Bearing LiMSSI Termini

All the polymers were synthesized following the method described for PEG200-LiMSSI2 (2.00 g, 10.0 mmol). The results are summarized in Table 1, and the 1H NMR spectra are indicated in the Supplementary Materials (Figures S1–S6).

3. Results and Discussion

3.1. Synthesis of PEGs with LiMSSI Termini

Through the concomitant Michael addition of the terminal hydroxy groups of PEG and lithiation, we synthesized PEGs with one LiMSSI terminus (PEGxMME-LiMSSI1) and two LiMSSI termini at both ends (PEGx-LiMSSI2) using PEG monomethyl ether and PEG with both terminal hydroxy groups, respectively, where x denotes the number-average molecular weight of PEG. Furthermore, a three-terminated oligo(ethylene glycol) TMPE450-LiMSSI3 and a diethylene glycol derivative bearing two LiMSSI termini at one end (DEGMME-LiMSSI2) were synthesized via the reaction of trimethylolpropane ethoxylate (average Mn = 450) (TMPE450) and DEGMME diol, respectively. An excess amount (1.0–1.5 equivalents) of MSVSI and an excess amount (2–3 equivalents) of lithium hydroxide monohydrate were added to the terminal hydroxyl group of each PEG, and the reaction was carried out at 100 °C for 48 h under a nitrogen atmosphere. If the introduction efficiencies were insufficient, the reaction was further carried out by adding an excess amount of MSVSI and lithium hydroxide monohydrate. Purification methods were adjusted based on the solubility of each polymer.
As an example, Figure 2a shows the 1H-NMR spectrum of PEG200-LiMSSI2, indicating a peak at 3.01 ppm derived from the methyl group of the methanesulfonyl group (a) and peaks at 3.42 (b) and 3.88 ppm (c) derived from the ethylene group adjacent to the sulfonyl group along with the peak of the PEG unit. The peak (f) derived from the methylene group adjacent to the hydroxyl group at 3.57 ppm is almost unobservable, indicating that the hydroxy group is almost completely consumed. The fact that the incorporation ratio was higher than 99% was confirmed by the integral ratio of the peak derived from the LiMSSI group to the peak derived from the PEG chain at 3.6 ppm. In addition, a peak at 2.96 ppm was observed in the 7Li-NMR spectrum, indicating the presence of lithium salt moieties (Figure 2b).

3.2. Properties of PEGs with LiMSSI Termini

3.2.1. Electrochemical Stability

The electrochemical stability of PEG200-LiMSSI2 was evaluated by CV measurements using EC/DEC (v/v = 3/7) containing 1.0 M of LiTFSI as the electrolyte solution, silver nitrate electrolyte as the reference electrode, a platinum disk as the working electrode, and a platinum wire as the counter electrode at a sweep rate of 0.1 V/s. The cyclic voltammogram of the electrolyte solutions of PEG200-LiMSSI2 (Figure 3) showed only peaks around 2.5 V and −3.5 V, originating from the oxidation and reduction of the electrolyte. None of the oxidation and reduction peaks of the polymers were observed, indicating that PEG200-LiMSSI2 is electrochemically stable enough in the electrochemical window of the electrolyte. The cyclic voltammograms of DEGMME-LiMSSI2 and TMPE450-LiMSSI3, which have different structures, were identical to that of PEG200-LiMSSI2, indicating their electrochemical stability (Figure S7).

3.2.2. Thermal Behaviors

The glass transition, crystallization, and melting behavior of the synthesized PEG-LiMSSI were analyzed using DSC. The analysis was performed in the second heating scan at a heating rate of 10 °C/min after the first heating scan to 100 °C, followed by the cooling scan to −80 °C at a cooling rate of 10 °C/min (Figure S8). The Tg and melting temperature (Tm) are summarized in Table 1.
The crystallization of the PEG chains was suppressed by the terminal LiMSSI structure as previously reported in PEG derivatives with anionic termini [6,7,8,9]. In the thermograms of PEGx-LiMSSI2 (x = 200, 400, and 1000) and PEGxMME-LiMSSI1 (x = 200 and 400), no endothermic peaks derived from the melting of PEG chain crystals were observed, indicating that the terminal LiMSSI structure completely suppressed the crystallization of PEG. DEGMME-LiMSSI2 and TMPE450-LiMSSI3, whose oligoethers are not crystalline, were also amorphous within the investigated temperature range. On the other hand, in the DSC curve of PEG1000MME-LiMSSI, an exothermic peak resulting from cold crystallization was observed at around −35 °C, and an endothermic peak resulting from the melting of PEG chains was observed at 27 °C. These data indicate that sufficient lengths of PEG chains, apart from the LiMSSI terminus, are necessary for crystallization.
The terminal LiMSSI structure increased the Tg through intermolecular ionic interactions. For the same molecular weight of PEG, the Tg was higher for the doubly terminated PEG. For example, the Tg of the mono-terminated PEG400MME-LiMSSI1 and the doubly terminated PEG400-LiMSSI2 with the quantitative introduction efficiency were −48 °C and −11 °C, respectively. The introduction efficiency also affects the Tg. We prepared PEG200-LiMSSI2 and PEG400-LiMSSI2 with different introduction efficiencies and found that the Tgs are increased by the quantitative introduction of the LiMSSI ends. The Tg of TPME450-LiMSSI3 is also higher than that of PEG400MME-LiMSSI1 and is identical to that of PEG400-LiMSSI2 with a closer introduction efficiency. Considering the lower introduction efficiency and higher molecular weight of TPME450-LiMSSI3, we suggest that the three ionic end groups in one molecule resulted in ionic cross-linkage, which restricts the movement of ions and ether chains.

3.2.3. Ionic Conductivity

The effects of PEG’s molecular weight, and the introduction efficiency, number, and morphological arrangement of the LiMSSI structure on the ionic conductivity were comprehensively evaluated by comparing the ionic conductivity. The ionic conductivity was measured at each temperature during cooling from 100 °C under nitrogen. Prior to measurement, the samples were annealed at 90 °C under reduced pressure for half a day and then brought to a steady state under nitrogen.
The effect of PEG’s molecular weight on ionic conductivity was evaluated by changing the PEG molecular weight (x) of PEGX-LiMSSI2 with LiMSSI structures at both ends to 200, 400, and 1000 (Figure 4).
The ionic conductivity of PEGx-LiMSSI2 (x = 200, 400, and 1000) with an introduction efficiency higher than 95% (filled marks in Figure 4) increased with an increasing PEG molecular weight. This trend is consistent with previously developed PEGs with ionic ends [6,7,8,9] and correlates with Tg. The LiMSSI structure is sterically stiffer than the PEG chain and forms ionic interactions. These structural and chemical factors both restrict the mobility of the polymer chains and thus reduce the mobility of the lithium ions.
The ionic conductivities of PEG200-LiMSSI2 and PEG400-LiMSSI2 with lower introduction efficiencies were also investigated (open marks in Figure 4). In both cases, the ionic conductivities were higher than those of the analogs with the higher introduction efficiencies. This effect of the introduction efficiency was striking. The approximately 5% decrease in the introduction efficiency decreased the ionic conductivity by three orders of magnitude, even though the [Li]/[O] ratios were almost identical. The Tgs also became significantly higher with the slight decrease in the introduction efficiency. This difference will be discussed later.
We compared the ionic conductivities of PEG400MME-LiMSSI, PEG400-LiMSSI2, and TMPE450-LiMSSI3 with one, two, and three terminal LiMSSI structures, respectively, with molecular weights of the PEG chains being approximately 400 to study the effect of different end groups (Figure 5).
The ionic conductivity decreased as the number of terminal LiMSSI groups increased. In particular, the trifunctional TMPE450-LiMSSI3 is more than two orders of magnitude lower than the monofunctional PEG400MME-LiMSSI and the difunctional PEG400-LiMSSI2. The Tg also increased as the number of terminal LiMSSI groups increased. As with the PEG molecular weights, the decrease in ionic conductivity and the increase in Tg were attributed to an increase in the [Li]/[O] ratio and the density of the terminal LiMSSI groups, resulting in more interchain interactions. Therefore, we compared the ionic conductivity of PEG200-LiMSSI2, which has a higher [Li]/[O] ratio than that of TMPE450-LiMSSI3. As a result, their ionic conductivities were almost equivalent. This result suggests that the significant factor in the decrease in ionic conductivity is the number of end groups rather than the increase in the [Li]/[O] ratio. With the interchain interactions of the terminal LiMSSi groups, the PEG with one LiMSSI end dimerizes, and the PEG with two end groups polymerizes. These constraints are two-dimensional and slightly limit segmental motion, thus maintaining low Tgs. In contrast, a PEG with three terminal LiMSSI groups forms a three-dimensional ionic cross-linkage, which constrains the entire molecule and increases the Tg, resulting in a significant decrease in ionic conductivity.
Finally, we compared the ionic conductivity of DEG-MME-LiMSSI2 with two LiMSSI structures at one end to that of PEG200-LiMSSI2 with a similar [Li]/[O] ratio to investigate the effect of the different arrangements of the terminal LiMSSI groups on the ionic conductivity (Figure 6). The one-sided, two-terminated DEGMME-LiMSSI2 had a lower ionic conductivity than the PEG200-LiMSSI2 with LiMSSI moieties at both ends, although the Tg was 34 K lower than that of PEG200-LiMSSI2. The low ionic conductivity of DEGMME-LiMSSI2 is probably due to the intramolecular interactions of the two terminal LiMSSI groups located within close positions. The low Tg relative to the high [Li]/[O] ratio implies a lower tendency for intermolecular interactions, which increases the freedom of chain motion. On the other hand, the intramolecular interaction between the terminal LiMSSI groups would confine the lithium ions within the molecule to suppress the intermolecular transfer of lithium ions.
The ion conductivities of the examined materials are summarized in Table 2, together with those of some previously reported single-component PEG-based electrolytes. However, an exact comparison between different reports is not possible since ion conductivities are severely influenced by absorbed water [18], and measurements without appropriate drying overestimate ion conductivities (Figure S9). The ionic conductivities of fluorine-free polyelectrolytes are mostly in the range of 10−6–10−7 S/cm at ambient temperature, while those of fluorine-containing polyelectrolytes are almost an order of magnitude higher. Our PEG-LiMSSI derivatives with lower Tgs are in a higher range among fluorine-free single-component polyelectrolytes. In contrast, the derivatives with higher Tgs, namely PEG-LiMSSI with multiple LiMSSI ends and a quantitative introduction efficiency, exhibited lower ionic conductivities.
The logarithms of the ionic conductivities of our materials at 60 °C correlate well with the Tgs, except for DEGMME-LiMSSI2 and TPME450-LiMSSI3, which have low ionic conductivities relative to their Tgs (Figure 7). The R2 values for the linear correlations are 0.42 and 0.80 for all the examined derivatives and the derivatives except DEGMME-LiMSSI2 and TPME450-LiMSSI3, respectively. This correlation implies that the ionic conduction in PEGxMME-LiMSSI1 and PEGx-LiMSSI2 proceeds in an identical mechanism. Intramolecular and three-dimensional ionic interactions negatively affected the ionic conduction behaviors.
Based on these results, we suggest PEGxMME-LiMSSI1 and PEGx-LiMSSI2 containing a trace amount of an unreacted end to improve the mobility of the chains as suitable single-component polyelectrolytes.

4. Conclusions

Fluorine-free single-component polyelectrolytes were developed by introducing LiMSSI moieties to PEG derivatives with one, two, and three LiMSSI termini via the simultaneous Michael-type addition and lithiation of PEGs and MSVSI. The ionic conductivities at 60 °C ranged from 1.8 × 10−7 to 2.0 × 10−4 S/cm. PEG-LiMSSI derivatives with one LiMSSI terminus (PEGxMME-LiMSSI1) and two LiMSSI termini at both ends (PEGx-LiMSSI2) exhibited higher ionic conductivity than those with two LiMSSI termini at one end (DEGMME-LiMSSI2) and with three LiMSSI termini (TPME450-LiMSSI3), and their ionic conductivities correlated well with their Tgs. The low ionic conductivities of DEGMME-LiMSSI2 and TPME450-LiMSSI3 probably result from the restriction of the mobility of lithium cation via intermolecular and networked ionic interactions, respectively. PEGxMME-LiMSSI1 and PEGx-LiMSSI show good ionic conductivity as fluorine-free single-component polyelectrolytes without additional salts and solvents.
This work revealed the effect of the structural variance of a series of PEG derivatives with anionic end moieties on ionic conductivities, which is informative for the design of single-component polyelectrolytes. The remaining task for the further optimization of our materials is the evaluation of the transference numbers of Li+, which are expected to be higher than 0.4, similar to that reported in polyelectrolytes due to the suppressed transport of anions. In addition, the suppression of intermolecular ionic interactions without intramolecular interactions will also lower the Tg and, thus, improve ionic conductivities. These investigations will contribute to the development of fluorine-free polyelectrolytes for sustainable electronics.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/technologies12050065/s1, Figures S1–S6: 1H NMR spectra of PEG-LiMSSI derivatives; Figure S7. Cyclic voltammograms of DEGMME-LiMSSI2 and TPME450-LiMSSI3; Figure S8: DSC curves of polyelectrolytes; Figure S9: ionic conductivity of PEG-LiMSSI with insufficient drying.

Author Contributions

Conceptualization, B.O.; methodology, B.O., K.H., Y.F. and Y.M.; software, B.O., K.H. and Y.F.; validation, B.O., K.H., Y.F. and Y.M.; formal analysis, K.H. and Y.F.; investigation, K.H. and Y.F.; resources, B.O. and Y.M.; data curation, B.O., K.H. and Y.F.; writing—original draft preparation, B.O., K.H. and Y.F.; writing—review and editing, B.O. and Y.M.; visualization, B.O., K.H. and Y.F.; supervision, B.O.; project administration, B.O.; funding acquisition, B.O. and Y.M. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All the data substantiating the conclusion of this study are included. Other primary data are available upon reasonable request from the corresponding author.

Acknowledgments

The authors are grateful to Hideharu Mori of Yamagata University for his kind assistance in ionic conductivity measurements.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Murata, K.; Izuchi, S.; Yoshihisa, Y. An overview of the research and development of solid polymer electrolyte batteries. Electrochim. Acta 2000, 45, 1501. [Google Scholar] [CrossRef]
  2. Xu, K. Electrolytes and interphases in Li-ion batteries and beyond. Chem. Rev. 2014, 114, 11503–11618. [Google Scholar] [CrossRef] [PubMed]
  3. Zhang, H.; Li, C.; Piszcz, M.; Coya, E.; Rojo, T.; Rodriguez-Martinez, L.M.; Armand, M.; Zhou, Z. Single lithium-ion conducting solid polymer electrolytes: Advances and perspectives. Chem. Soc. Rev. 2017, 46, 797–815. [Google Scholar] [CrossRef]
  4. Tong, B.; Song, Z.; Wu, H.; Wang, X.; Feng, W.; Zhou, Z.; Zhang, H. Ion transport and structural design of lithium-ion conductive solid polymer electrolytes: A perspective. Mater. Futures 2022, 1, 042103. [Google Scholar] [CrossRef]
  5. Ohno, H.; Ito, K. Poly(ethylene oxide)s having carboxylate groups on the chain end. Polymer 1995, 36, 891–893. [Google Scholar] [CrossRef]
  6. Ito, K.; Tominaga, Y.; Ohno, H. Polyether/salt hybrid (IV). Effect of benzenesulfonate group(s) and PEO molecular weight on the bulk ionic conductivity. Electrochim. Acta 1997, 42, 1561–1570. [Google Scholar] [CrossRef]
  7. Ito, K.; Nishina, N.; Ohno, H. High lithium ionic conductivity of poly(ethylene oxide)s having sulfonate groups on their chain ends. J. Mater. Chem. 1997, 7, 1357–1362. [Google Scholar] [CrossRef]
  8. Tominaga, Y.; Ohno, H. High ionic conductivity of PEO/sulfonamide salt hybrids. Solid State Ion. 1999, 124, 323–329. [Google Scholar] [CrossRef]
  9. Tominaga, Y.; Ohno, H. Lithium ion conduction in linear- and network-type polymers of PEO/sulfonamide salt hybrids. Electrochim. Acta 2000, 45, 3081–3086. [Google Scholar] [CrossRef]
  10. Fujinami, T.; Buzoujima, Y. Novel lithium salts exhibiting high lithium ion transference numbers in polymer electrolytes. J. Power Sources 2003, 119–121, 438–441. [Google Scholar] [CrossRef]
  11. Shobukawa, H.; Tokuda, H.; Tabata, S.; Watanabe, M. Preparation and transport properties of novel lithium ionic liquids. Electrochim. Acta 2004, 50, 305–309. [Google Scholar] [CrossRef]
  12. Zygadło-Monikowska, E.; Florjańczyk, Z.; Ostrowska, J.; Bołtromiuk, P.; Frydrych, J.; Sadurski, W.; Langwald, N. Synthesis and characterization of new trifluoroalkoxyborates lithium salts of ionic liquid properties. Electrochim. Acta 2011, 57, 66–73. [Google Scholar] [CrossRef]
  13. Zygadło-Monikowska, E.; Florjańczyk, Z.; Służewska, K.; Ostrowska, J.; Langwald, N.; Tomaszewska, A. Lithium conducting ionic liquids based on lithium borate salts. J. Power Sources 2010, 195, 6055–6061. [Google Scholar] [CrossRef]
  14. Zygadło-Monikowska, E.; Florjańczyk, Z.; Tomaszewska, A.; Pawlicka, M.; Langwald, N.; Kovarsky, R.; Mazor, H.; Golodnitsky, D.; Peled, E. New boron compounds as additives for lithium polymer electrolytes. Electrochim. Acta 2007, 53, 1481–1489. [Google Scholar] [CrossRef]
  15. Guzmán-González, G.; Alvarez-Tirado, M.; Olmedo-Martínez, J.L.; Picchio, M.L.; Casado, N.; Forsyth, M.; Mecerreyes, D. Lithium borate ionic liquids as single-component electrolytes for batteries. Adv. Energy Mater. 2023, 13, 2202974. [Google Scholar] [CrossRef]
  16. Hallac, B.B.; Geiculescu, O.E.; Rajagopal, R.V.; Creager, S.E.; DesMarteau, D.D. Lithium-conducting ionic melt electrolytes from polyether-functionalized fluorosulfonimide anions. Electrochim. Acta 2008, 53, 5985–5991. [Google Scholar] [CrossRef]
  17. Herath, M.B.; Creager, S.E.; Rajagopal, R.V.; Geiculescu, O.E.; DesMarteau, D.D. Ionic conduction in polyether-based lithium arylfluorosulfonimide ionic melt electrolytes. Electrochim. Acta 2009, 54, 5877–5883. [Google Scholar] [CrossRef]
  18. Flachard, D.; Rolland, J.; Obadia, M.M.; Serghei, A.; Bouchet, R.; Drockenmuller, E. A 1,2,3-triazolate lithium salt with ionic liquid properties at room temperature. Chem. Commun. 2018, 54, 9035–9038. [Google Scholar] [CrossRef] [PubMed]
  19. Feng, S.W.; Shi, D.Y.; Liu, F.; Zheng, L.P.; Nie, J.; Feng, W.F.; Huang, X.J.; Armand, M.; Zhou, Z.B. Single lithium-ion conducting polymer electrolytes based on poly[(4-styrenesulfonyl)(trifluoromethanesulfonyl)imide] anions Electrochim. Acta 2013, 93, 254–263. [Google Scholar]
  20. Bouchet, R.; Maria, S.; Meziane, R.; Aboulaich, A.; Lienafa, L.; Bonnet, J.-P.; Phan, T.N.T.; Bertin, D.; Gigmes, D.; Devaux, D.; et al. Single-ion BAB triblock copolymers as highly efficient electrolytes for lithium-metal batteries. Nat. Mater. 2013, 12, 452–457. [Google Scholar] [CrossRef]
  21. Ma, Q.; Zhang, H.; Zhou, C.; Zheng, L.; Cheng, P.; Nie, J.; Feng, W.; Hu, Y.-S.; Li, H.; Huang, X.; et al. Single lithium-ion conducting polymer electrolytes based on a super-delocalized polyanion. Angew. Chem. Int. Ed. 2016, 55, 2521–2525. [Google Scholar] [CrossRef]
  22. Matsumoto, K.; Endo, T. Design and synthesis of ionic-conductive epoxy-based networked polymers. React. Funct. Polym. 2013, 73, 278–282. [Google Scholar] [CrossRef]
  23. Ankley, G.T.; Cureton, P.; Hoke, R.A.; Houde, M.; Kumar, A.; Kurias, J.; Lanno, R.; McCarthy, C.; Newsted, J.; Salice, C.J.; et al. Assessing the Ecological risks of per- and polyfluoroalkyl substances: Current state-of-the science and a proposed path forward. Environ. Toxicol. Chem. 2021, 40, 564–605. [Google Scholar] [CrossRef] [PubMed]
  24. Brunn, H.; Arnold, G.; Körner, W.; Rippen, G.; Steinhäuser, K.G.; Valentin, I. PFAS: Forever chemicals—Persistent, bioaccumulative and mobile. Reviewing the status and the need for their phase out and remediation of contaminated sites. Environ. Sci. Eur. 2023, 35, 20. [Google Scholar] [CrossRef]
  25. Mandal, B.; Sooksimuang, T.; Griffin, B.; Padhi, A.; Filler, R. New lithium salts for rechargeable battery electrolytes. Solid State Ion. 2004, 175, 267–272. [Google Scholar] [CrossRef]
  26. Scheers, J.; Lim, D.-H.; Kim, J.-K.; Paillard, E.; Henderson, W.A.; Johansson, P.; Ahn, J.-H.; Jacobsson, P. All fluorine-free lithium battery electrolytes. J. Power Sources 2014, 251, 451–458. [Google Scholar] [CrossRef]
  27. Hosseini-Bab-Anari, E.; Boschin, A.; Mandai, T.; Masu, H.; Moth-Poulsen, K.; Johansson, P. Fluorine-free salts for aqueous lithium-ion and sodium-ion battery electrolytes. RSC Adv. 2016, 6, 85194–85201. [Google Scholar] [CrossRef]
  28. He, X.; Yan, B.; Zhang, X.; Liu, Z.; Bresser, D.; Wang, J.; Wang, R.; Cao, X.; Su, Y.; Jia, H.; et al. Fluorine-free water-in-ionomer electrolytes for sustainable lithium-ion batteries. Nat. Commun. 2018, 9, 5320. [Google Scholar] [CrossRef]
  29. Martinez-Ibañez, M.; Sanchez-Diez, E.; Qiao, L.; Meabe, L.; Santiago, A.; Zhu, H.; O’Dell, L.A.; Carrasco, J.; Forsyth, M.; Armand, M.; et al. Weakly coordinating fluorine-free polysalt for single lithium-ion conductive solid polymer electrolytes. Batter. Supercaps 2020, 3, 738–746. [Google Scholar] [CrossRef]
  30. Hernández, G.; Mogensen, R.; Younesi, R.; Mindemark, J. Fluorine-free electrolytes for lithium and sodium batteries. Batter. Supercaps 2022, 5, e202100373. [Google Scholar] [CrossRef]
  31. Matsumura, Y.; Shiraiwa, T.; Hayasaka, T.; Yoshida, S.; Ochiai, B. Synthesis of fluorine-free highly ion conductive polymer electrolyte having lithium bissulfonimide unit. J. Electrochem. Soc. 2018, 165, B3119–B3121. [Google Scholar] [CrossRef]
  32. Nakatsuji, Y.; Nakamura, T.; Okahara, M.; Dishong, D.M.; Gokel, G.W. Crown cation complex effects. 22. Enhancement of cation binding in lariat ethers bearing a methyl group at the quaternary, pivot carbon atom. J. Org. Chem. 1983, 48, 1237–1242. [Google Scholar] [CrossRef]
  33. Cowie, J.; Spence, G. Novel single ion, comb-branched polymer electrolytes. Solid State Ion. 1999, 123, 233–242. [Google Scholar] [CrossRef]
Figure 1. The PEGs with LiMSSI termini examined in this study.
Figure 1. The PEGs with LiMSSI termini examined in this study.
Technologies 12 00065 g001
Figure 2. (a) The 1H NMR spectra of MSVSI, PEG200, and PEG200-LiMSSI2 (400 MHz); and the (b) 7Li NMR spectrum of PEG200-LiMSSI2 (194 MHz) (D2O).
Figure 2. (a) The 1H NMR spectra of MSVSI, PEG200, and PEG200-LiMSSI2 (400 MHz); and the (b) 7Li NMR spectrum of PEG200-LiMSSI2 (194 MHz) (D2O).
Technologies 12 00065 g002
Figure 3. Cyclic voltammograms of PEG200-LiMSSI2 (plain) and background (dashed) in a 1.0 M EC/DEC (v/v = 3/7) solution of LiTFSI; reference electrode, Ag/Ag+; working electrode, Pt disk (φ = 1.6 mm); counter electrode, Pt wire (φ = 0.5 mm); sweep rate = 0.1 V/s.
Figure 3. Cyclic voltammograms of PEG200-LiMSSI2 (plain) and background (dashed) in a 1.0 M EC/DEC (v/v = 3/7) solution of LiTFSI; reference electrode, Ag/Ag+; working electrode, Pt disk (φ = 1.6 mm); counter electrode, Pt wire (φ = 0.5 mm); sweep rate = 0.1 V/s.
Technologies 12 00065 g003
Figure 4. The ionic conductivity of PEG200-LiMSSI2 (red triangle) with an LiMSSI introduction efficiency of 95% (opened) and >99% (filled), PEG400-LIMSSI2 (green circle) with an LiMSSI introduction efficiency of 91% (opened) and >99% (filled), and PEG1000-LiMSSI2 with an LiMSSI introduction efficiency of >99% (blue square).
Figure 4. The ionic conductivity of PEG200-LiMSSI2 (red triangle) with an LiMSSI introduction efficiency of 95% (opened) and >99% (filled), PEG400-LIMSSI2 (green circle) with an LiMSSI introduction efficiency of 91% (opened) and >99% (filled), and PEG1000-LiMSSI2 with an LiMSSI introduction efficiency of >99% (blue square).
Technologies 12 00065 g004
Figure 5. The ionic conductivities of PEG400-MME-LiMSSI (blue square), PEG400-LiMSSI2 (green circle), and TMPE450-LiMSSI3 (red triangle).
Figure 5. The ionic conductivities of PEG400-MME-LiMSSI (blue square), PEG400-LiMSSI2 (green circle), and TMPE450-LiMSSI3 (red triangle).
Technologies 12 00065 g005
Figure 6. The ionic conductivities of DEG-MME-LiMSSI2 (green circle) and PEG200-LiMSSI2 (red triangle).
Figure 6. The ionic conductivities of DEG-MME-LiMSSI2 (green circle) and PEG200-LiMSSI2 (red triangle).
Technologies 12 00065 g006
Figure 7. The ionic conductivities of the PEG-LiMSSI derivatives in this study. Mono-LiMSSI terminal (green circle), both-end type two LiMSSI termini (blue square), single-end type two LiMSSI termini (purple rhombus), and three LiMSSI termini (red triangle) PEG derivatives.
Figure 7. The ionic conductivities of the PEG-LiMSSI derivatives in this study. Mono-LiMSSI terminal (green circle), both-end type two LiMSSI termini (blue square), single-end type two LiMSSI termini (purple rhombus), and three LiMSSI termini (red triangle) PEG derivatives.
Technologies 12 00065 g007
Table 1. The LiMSSI-terminated PEG examined in this research.
Table 1. The LiMSSI-terminated PEG examined in this research.
PolymerPEGIntroduction Efficiency (%) a[Li]/[O] bYield (%)Tg (°C) cTm (°C) c
PEG400MME-LiMSSI1PEG400MME>990.1045 d−48n.o.h
PEG1000MME-LiMSSI1PEG1000MME950.04550 d−5627
PEG200-LiMSSI2PEG200950.46ca. 40 d,e−18n.o.h
>990.4834 d9n.o.h
PEG400-LiMSSI2PEG400910.1970 d−30n.o.h
>990.21ca. 15 d,e−11n.o.h
PEG1000-LiMSSI2PEG1000>990.08270 d−18n.o.h
DEGMME-LiMSSI2DEGMME-diol890.3612 f−52n.o.h
TMPE450-LiMSSI3TPME450860.3025 g−18n.o.h
a Determined via 1H NMR spectroscopy (400 MHz, D2O). b Molar ratio of Li to O in ethylene glycol units (the O in the sulfonimide structures was omitted from the calculation). c Determined by DSC (10 °C/min, second heating scan, N2). d The isolated yield after reprecipitation with ethyl acetate from an ethanol solution. e The approximate value due to loss during the repeated confirmation of introduction efficiency. f The isolated yield after reprecipitation with ethyl acetate from a THF solution. g The isolated yield after reprecipitation with CH2Cl2 from an acetone solution. h Not observed.
Table 2. The ionic conductivities of the LiMSSI-terminated PEG examined in this research and the reported polymeric electrolytes bearing anionic structures.
Table 2. The ionic conductivities of the LiMSSI-terminated PEG examined in this research and the reported polymeric electrolytes bearing anionic structures.
CategoryPolymerIE (%) aσtotal (S/cm)Tg (°C)Ref
F-freePEG400MME-LiMSSI1>995.5 × 10−6 @ 30 °C
1.1 × 10−4 @ 60 °C
−48This work
PEG1000MME-LiMSSI1953.0 × 10−5 @ 30 °C
2.0 × 10−4 @ 60 °C
−56This work
PEG200-LiMSSI2951.3 × 10−6 @ 30 °C
7.8 × 10−5 @ 60 °C
−18This work
>991.8 × 10−7 @ 60 °C9This work
PEG400-LiMSSI2912.3 × 10−7 @ 30 °C
4.1 × 10−5 @ 60 °C
−30This work
>998.1 × 10−8 @ 30 °C
1.2 × 10−5 @ 60 °C
−11This work
PEG1000-LiMSSI2>992.5 × 10−6 @ 30 °C
5.2 × 10−5 @ 60 °C
−18This work
DEGMME-LiMSSI2897.3 × 10−7 @ 30 °C
4.5 × 10−5 @ 60 °C
−52This work
TMPE450-LiMSSI3862.7 × 10−7 @ 60 °C−18This work
PEG350-(SO3Li)1N/A4.45 × 10−6 @ 30 °C−53[7]
PEG600-(SO3Li)2N/A1.43 × 10−6 @ 30 °C−31[7]
PEG550-SO2N(Li)CH2CH2OCH3N/A2.5 × 10−5 @ 30 °Cnot reported[8]
PEG1900-(SO2N(Li)Ph)2N/A1.08 × 10−6 @ 30 °C
3.23 × 10−6 @ 50 °C
Semi-crystalline (Tm = 27 °C)[9]
Networked PEG2000-SO2N(Li)PhN/A1.40 × 10−6 @ 30 °C
4.34 × 10−6 @ 50 °C
Rubbery
(Tm = 34 °C)
[9]
MeO(CH2CH2O)3CH2-1,2,3-triazolateN/A8.0 × 10−7 @ 30 °C−60 >[18]
Li{B[O(CH2CH2O)nCH3]3C4H9}N/A2 × 10−5 @ 30 °C−79[13]
Poly(LiMSVSI-co-PEGMA)N/A8.4 × 10−5 @ 25 °C
9.2 × 10−4 @ 70 °C
−62[31]
F-containingLi+{Al[(OCH2CH2)nOMe]2(SO2CF3)2]
(n = 11.8)
N/A4.9 × 10−5 @ 30 °C−53[10]
Li+{B[(OCH2CH2)4OMe]2HFIP2}N/A4.6 × 10−6 @ 30 °C−54[11]
MeOPEG550OCF2CFHOCF2CF2SO2N(Li)SO2CF3N/A5.3 × 10−6 @ 30 °Cnot reported[16]
MeO(CH2CH2O)12C6H4SO2N(Li)SO2CF3N/A7.1 × 10−6 @ 30 °C−38[17]
Li+{B[(OCH2CH2)3OMe]2-HFIP-But}N/A1.89 × 10−4 @ 25 °Cnot reported
(liquid)
[15]
P(EOMA-co-FBSALi)N/A4.0 × 10−4 @ 30 °C−51[33]
P(LiSTFSI-co-MPEGA)N/A7.7 × 10−6 @ 25 °C
1.0 × 10−4 @ 60 °C
−47[19]
LiPSTFSI-b-PEO-b-LiPSTFSIN/A1.3 × 10−5 @ 60 °C−25[20]
a Introduction efficiency calculated using 1H NMR spectroscopy. Abbreviations: HFIP, hexafluoroisopropoxy; P(EOMA-co-FBSALi), poly(ethylene oxide methoxy acrylate-co-lithium 1,1,2-trifluorobutanesulfonate acrylate); LiSTFSI, lithium (4-styrenesulfonyl)(trifluoromethanesulfonyl imide); MPEGA, methoxy polyethylene glycol acrylate; LiPSTFSI, lithium(4-styrenesulfonyl)(trifluoromethyl(S-trifluoromethylsulfonylimino) sulfonyl)imide; N/A, not available.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Ochiai, B.; Hirabayashi, K.; Fujii, Y.; Matsumura, Y. Fluorine-Free Single-Component Polyelectrolyte of Poly(ethylene glycol) Bearing Lithium Methanesulfonylsulfonimide Terminal Groups: Effect of Structural Variance on Ionic Conductivity. Technologies 2024, 12, 65. https://doi.org/10.3390/technologies12050065

AMA Style

Ochiai B, Hirabayashi K, Fujii Y, Matsumura Y. Fluorine-Free Single-Component Polyelectrolyte of Poly(ethylene glycol) Bearing Lithium Methanesulfonylsulfonimide Terminal Groups: Effect of Structural Variance on Ionic Conductivity. Technologies. 2024; 12(5):65. https://doi.org/10.3390/technologies12050065

Chicago/Turabian Style

Ochiai, Bungo, Koki Hirabayashi, Yudai Fujii, and Yoshimasa Matsumura. 2024. "Fluorine-Free Single-Component Polyelectrolyte of Poly(ethylene glycol) Bearing Lithium Methanesulfonylsulfonimide Terminal Groups: Effect of Structural Variance on Ionic Conductivity" Technologies 12, no. 5: 65. https://doi.org/10.3390/technologies12050065

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop