Surface Ligand Influences the Cu Nanoclusters as a Dual Sensing Optical Probe for Localized pH Environment and Fluoride Ion
Next Article in Special Issue
Effect of Doping TiO2 NPs with Lanthanides (La, Ce and Eu) on the Adsorption and Photodegradation of Cyanide—A Comparative Study
Previous Article in Journal
Cobalt-Phosphate (Co-Pi)-Modified WO3 Photoanodes for Performance-Enhanced Photoelectrochemical Wastewater Degradation
Previous Article in Special Issue
Time-Dependent Size and Shape Evolution of Gold and Europium Nanoparticles from a Bioproducing Microorganism, a Cyanobacterium: A Digitally Supported High-Resolution Image Analysis
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Influence of SiO2 Embedding on the Structure, Morphology, Thermal, and Magnetic Properties of Co0.4Zn0.4Ni0.2Fe2O4 Particles

1
Faculty of Science, Technical University of Cluj-Napoca, 76 Victoriei Street, 430122 Baia Mare, Romania
2
INCDO-INOE 2000, Research Institute for Analytical Instrumentation, 67 Donath Street, 400293 Cluj-Napoca, Romania
3
Faculty of Physics, Babes-Bolyai University, 1 Kogalniceanu Street, 400084 Cluj-Napoca, Romania
4
National Institute for Research and Development of Isotopic and Molecular Technologies, 67-103 Donath Street, 400293 Cluj-Napoca, Romania
*
Author to whom correspondence should be addressed.
Nanomaterials 2023, 13(3), 527; https://doi.org/10.3390/nano13030527
Submission received: 20 December 2022 / Revised: 23 January 2023 / Accepted: 26 January 2023 / Published: 28 January 2023

Abstract

:
(Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)(100−α) samples obtained by embedding Co0.4Zn0.4Ni0.2Fe2O4 nanoparticles in SiO2 in various proportions were synthesized by sol-gel process and characterized using thermal analysis, Fourier-transform infrared spectroscopy, X-ray diffraction, transmission electron microscopy, inductively coupled plasma optical emission spectrometry, and magnetic measurements. Poorly crystalline Co–Zn–Ni ferrite at low annealing temperatures (500 °C) and highly crystalline Co–Zn–Ni ferrite together with traces of crystalline Fe2SiO4 (800 °C) and SiO2 (tridymite and cristobalite) (1200 °C) were obtained. At 1200 °C, large spherical particles with size increasing with the ferrite content (36–120 nm) were obtained. Specific surface area increased with the SiO2 content and decreased with the annealing temperature above 500 °C. Magnetic properties were enhanced with the increase in ferrite content and annealing temperature.

1. Introduction

Spinel ferrite nanoparticles are widely studied due to their outstanding electrical and magnetic properties, high thermal and chemical stability, and applicability in different areas such as electronic, microwave, and communication devices, information storage systems, ferrofluid technology, solid oxide fuel cell, gas sensors, magnetocaloric refrigeration, and medical diagnosis [1,2,3,4]. The physicochemical properties of ferrites are determined by the preparation method, heat treatment, and chemical composition, as well as the type, stoichiometric ratio, and distribution of cations [5,6,7,8,9]. The particle morphology and surface coating may also influence the magnetic behavior of ferrites having the same compositions [10].
The synthesis route is a key factor in high-purity spinel ferrite nanoparticles’ preparation [5,9,11]. The most common ways to synthesize nanostructured ferrites are sol-gel, solid-phase, hydrothermal, coprecipitation, auto combustion, sonochemical, microwave refluxing, etc. [7,10,11]. The solid-state synthesis produces nanoparticles with high yields and well-controllable grain size [3]. At the same time, the conventional ceramic method produces particles in the micrometer range that tend to agglomerate due to slow reaction kinetics [11]. Generally, wet chemical synthesis methods such as hydrothermal, sol-gel, and auto combustion are used to produce high-purity crystalline ferrite nanoparticles at low annealing temperatures [2,3,11]. The sol-gel process allows the easy, low-cost production of ferrite nanocomposites with controlled structure and properties [12]. Moreover, the sol-gel process may produce nanocomposite materials comprising highly dispersed magnetic ferrite nanoparticles [13,14,15,16]. This method consists of incorporating metal nitrates in tetraethyl orthosilicate (TEOS), polycondensation of the SiO2 network, thermal-assisted formation of metal-carboxylate precursors in the reaction between the metal ions and diol, and thermal decomposition of carboxylate precursors into a hybrid oxidic system [14,15,16].
In the soft ferrites family, ZnFe2O4 is a spinel, with tetrahedral (A) sites occupied by Zn2+ ions and octahedral (B) sites by Fe3+ ions; NiFe2O4 is an inverse spinel, with Ni2+ ions occupying the octahedral (B) sites and Fe3+ ions equally distributed between octahedral (B) and tetrahedral (A) sites; whereas CoFe2O4 is a mixed spinel with high inversion degree [6]. The high electrical resistivity of NiFe2O4 is due to the lack of electron hopping, as Ni exists only in the divalent form [6]. By partial substitution of Ni2+ with Zn2+ in NiFe2O4, the Zn2+ ions will occupy the tetrahedral (A) sites, forcing the Fe3+ ions to occupy both octahedral (B) and tetrahedral (A) sites. This arrangement of the cations will increase the saturation magnetization (MS) of Ni–Zn ferrite, compared to that of NiFe2O4 and ZnFe2O4 [6,10,17]. Hence, by varying the substitution degree of the divalent cation, the magnetic behavior of Ni-Zn ferrites can be enhanced, making them fit for a broad range of applications [2,6,17,18]. Besides the high MS, Ni–Zn ferrites also present large electrical resistivity, narrow dielectric loss, low coercivity, good mechanical hardness, high magnetic permeability, and high operating frequency, which make them potential candidates for transformer cores, microwave devices, noise filters, recording heads, magnetic fluids, chokes, coils, etc., [2,3,4,7].
Ni–Zn ferrite has an inverse spinel structure with Fe3+ ions occupying both tetrahedral (A) and octahedral (B) sites, Ni2+ ions preferably located in octahedral (B) sites, and Zn2+ ions in tetrahedral (A) sites [3]. Adding Co2+ to Ni–Zn ferrite induces magnetic anisotropy and reduces the permeability due to the preferential orientation of the Co2+ ions’ magnetic moment along a particular direction [6,7]. The low dielectric loss, low magnetic loss, high saturation magnetizations, and high resistivity of mixed Co–Zn–Ni ferrites make them widely used as capacitors, filters, magnetic antennas, and absorbing materials [5,19,20].
The SiO2 embedding is used to control the particle size, reduce the particle agglomeration, and enhance the ferrites’ magnetic properties and biocompatibility, as SiO2 is biologically inert and diminishes the inflammatory risk [12,14]. One of the most used network-forming agents in sol-gel synthesis is TEOS, as it has a short gelation time, produces strong networks with moderate reactivity, and allows the embedding of both organic and inorganic molecules [14,15,16]. Previous studies demonstrated that transitional metal ferrites embedded in the SiO2 matrix display high magnetocrystalline anisotropy, unique magnetic structure, and high correlation between the coercivity, crystallite sizes, and annealing temperature [14,15,16]. Also, the partial substitution of Zn2+ ions by Co2+ ions in Zn–Ni ferrite was expected to enhance the magnetic properties of the nanoparticles.
This study investigates the relationship between the Co0.4Zn0.4Ni0.2Fe2O4 content embedded in the SiO2 matrix and the crystallite size, specific surface area, porosity particle size, thermal behavior, and magnetic properties (saturation magnetization–MS, remanent magnetization–MR, coercive field–Hc, magnetic anisotropy–K), and the Co0.4Zn0.4Ni0.2Fe2O4 content in the SiO2 matrix, at different annealing temperatures.

2. Materials and Methods

All chemical reagents were of analytical grade and were purchased from Merck (Darmstadt, Germany). (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)(100−α) samples were produced by sol-gel process dissolving Co(NO3)2∙6H2O, Zn(NO3)2·6H2O, Ni(NO3)2∙6H2O, and Fe(NO3)3∙9H2O in 1,3-propanediol (1,3PD), in a molar ratio of 0.4:0.4:0.2:2:8. Afterwards, TEOS dissolved in ethanol was added to the nitrate-1,3PD mixture, using 0:2 (α = 0%), 0.5:1.5 (α = 25%), 1:1 (α = 50%), 1.5:0.5 (α = 75%), and 2:0 (α = 100%) NO3:TEOS molar ratio. Diluted nitric acid was slowly added till the reaction mixture reached pH = 2 and then, the mixture was thoroughly stirred for 1 h. The obtained samples were dried at 40 °C for 5 h and 300 °C for 5 h, powdered in an agate mortar and annealed for 5 h at 500, 800, and 1200 °C, respectively, using an LT9 muffle furnace (Nabertherm, Lilienthal, Germany).
The thermal behavior of samples was studied by thermogravimetry (TG) and differential thermal analysis (DTA) by using a Q600 SDT (TA Instruments, New Castle, DE, USA) thermal analyzer, in air, up to 1200 °C, with a 10 °C/min- heating rate using an SDT Q600 thermogravimeter and alumina standards. A D8 Advance (Bruker, Karlsruhe, Germany) diffractometer equipped with a LynxEye linear detector was used for the investigation of crystalline phases, using the CuKα radiation (λ = 1.54060 Å) in the 2θ range 10–80°. The FT-IR spectra of the samples were recorded using a Spectrum BX II (Perkin Elmer, Waltham, MA, USA) Fourier-transform infrared (FT-IR) spectrometer, while the composition of Ni-Zn-Co ferrites was confirmed by Perkin Elmer Optima 5300 DV (Norwalk, CT, USA) inductively coupled plasma optical emission spectrometry (ICP-OES) after aqua regia digestion using a Speedwave Xpert (Berghof, Germany) microwave digestion system. N2 adsorption-desorption isotherms were recorded at −196 °C by a Sorptomatic 1990 (Thermo Fisher Scientific, Waltham, MA, USA) instrument, which was used for calculation of the specific surface area (SSA) using the Brunauer–Emmett–Teller (BET) model. The particle morphology was investigated using a transmission electron microscope (TEM, HD-2700, Hitachi, Tokyo, Japan) and a digital image recording system on samples deposited on carbon-coated copper grids. The average particle size was estimated from TEM measurements using the UTHSCSA ImageTool image software for over 100 nanoparticles in each sample. The hysteresis loops were recorded in magnetic fields between −2 to 2 T, at room temperature, and magnetization versus applied field was measured on samples embedded in an epoxy matrix by a 7400 vibrating-sample magnetometer (VSM, Lake Shore Cryotronics, Westerville, OH, USA). The magnetic measurement uncertainty was 10%.

3. Results and Discussion

The TG (Figure 1a) and DTA curves (Figure 1b indicates the maximum of the exothermic and endothermic effects, respectively) of sample α = 0% dried at 40 °C show two weak endothermic effects at 64 and 173 °C attributed to the loss of water from TEOS and an intense exothermic effect at 300 °C ascribed to 1,3PD decomposition [12]. These two processes result in a mass loss of 63.8% [12,15,16].
For samples α = 25, 50, 75, and 100%, the total mass loss slightly decreases (58.6–55.3%) with the Co0.4Zn0.4Ni0.2Fe2O4 content embedded in the SiO2 matrix. The formation of Co, Zn, and Ni malonates is indicated by the endothermic effect at 137–139 °C, whereas the formation of Fe malonate is indicated by the exothermic effect at 189–203 °C [12,14,15,16]. The exothermic effects at 278–292 °C are attributed to Co, Zn, and Ni malonates’ decomposition, while those at 321–325 °C are attributed to Fe malonates’ decomposition [12,14,15,16]. The temperature corresponding to the formation of divalent metal (Co, Ni, Zn) malonates slightly increases, whereas that of trivalent metal (Fe) malonates slightly decreases [12,14,15,16]. The transformations of the SiO2 matrix during the thermal process make it challenging to delimitate the effects ascribed to malonate precursors’ formation and decomposition [12,14,15,16].
Except for sample α = 0%, the FT-IR spectra of samples dried at 40 °C (Figure 2a) show a band at around 1380 cm−1, characteristic of nitrates. This band is missing for the samples heated at 300 °C, confirming the metal malonates’ formation and nitrates’ decomposition up to 300 °C [12,15,16]. For samples dried at 40 °C, the band at 1590–1620 cm−1 is specific to O–H vibrations in 1,3PD and adsorbed molecular water, and the bands at around 2950 and 2870 cm−1 are specific to stretching vibration of C-H in the methylene groups of 1,3PD. This band does not appear in the FT-IR spectra of samples annealed at high temperatures, indicating the precursor’s decomposition [15,16,21].
In the FT-IR spectra of sample α = 25–100% heated at 300 °C (Figure 2b), the band at around 1620 cm−1 characteristic to C=O of COO– groups’ vibration indicates the formation of malonate-metal complexes [15,16,21]. For samples α = 25–100%, the bands at 585–590 and 440–445 cm−1 indicate the presence of M-O bonds in tetrahedral (A) and octahedral (B) sites, respectively [15,16,21]. For samples α = 0–75% heated both at 40 and 300 °C, the characteristic bands for Si–O (440–445 cm−1) and Si–O–Si (1170–1200, 1056–1060, 792–829, 797–800, 585–590 cm−1) vibration suggests the formation of the SiO2 matrix [12,15,21]. The bands at 3420–3410 cm−1 are attributed to the vibration of O-H and hydrogen bonds in 1,3PD (40 °C) and metal malonates (300 °C) [15,16].
For sample α = 100% annealed at 300 °C (Figure 2c), the presence of well-defined, single-phase Co0.4Zn0.4Ni0.2Fe2O4 containing low-crystallized CoFe2O4 (JCPDS card no. 22–1086), ZnFe2O4 (JCPDS card no. 70–6491), and NiFe2O4 (JCPDS card no. 74–2081) is observed. The peaks pointed out at 2θ values of 18.29, 30.08, 35.43, 37.05, 43.05, 53.05, 56.97, 62.58, 70.95, 74.01, 75.01, 78.97° (CoFe2O4); 18.25, 30.01, 35.35, 36.98, 42.96, 53.30, 56.81, 62.39, 70.77, 73.79, 74.80, 78.74° (ZnFe2O4); and 18.42, 30.29, 35.68, 37.33, 43.37, 53.82, 57.37, 63.01, 71.51, 74.57, 75.58, 79.59° (NiFe2O4), corresponding to Miller indices of (111), (220), (311), (222), (400), (422), (511), (440), (620), (533), (622), and (444) confirms the formation of single-phase spinel-like structure (space group Fd3m). The degree of crystallinity was calculated using the highest intensity peak of spinel ferrite (311) [8,21,22]. In sample α = 75% annealed at 300 °C, the presence of Co0.4Zn0.4Ni0.2Fe2O4 is also observed, although the degree of crystallinity is lower than in sample α = 100%. In samples with low ferrite content α = 0, 25, and 50%, the crystalline ferrite is not remarked; the intensity of halo between 16 and 30° (2θ) ascribed to the amorphous SiO2 matrix increases with the SiO2 content.
Figure 3 displays the FT-IR spectra (left) and XRD patterns (right) of samples annealed at 500, 800, and 1200 °C. For samples α = 0–75%, the occurrence of SiO2 matrix is supported by the symmetric and asymmetric stretching vibrations of SiO4 tetrahedron (794–796 cm−1), the Si–O–Si stretching vibrations (1067–1093 cm−1), the shoulder at 1220–1250 cm−1 and the Si–O bond vibration (458–482 cm−1) [12,15,16]. These bands are lacking for samples α = 100%, the bands at 578–584 cm−1 being ascribed to Zn–O, Co–O and Ni–O vibrations, and at around 400 cm−1, they are ascribed to Fe–O bonds’ vibration [12,15,16]. For samples with high SiO2 content (α = 25%) annealed at 1200 °C, the vibration band at 620 cm−1 is attributed to Si–O–Si cyclic structures [12,15,16].
The XRD patterns of samples α = 100% annealed at 500, 800, and 1200 °C (Figure 3) display no impurities or unreacted Fe, Ni, Co, and Zn oxides, the broadening of diffraction peaks being ascribed to ultrafine Co0.4Zn0.4Ni0.2Fe2O4 particles [12,15,16]. The intensity of diffraction peaks matching to ferrites increases at high annealing temperatures indicating a high degree of crystallinity, high crystal nucleation (owing to the small growth rate and homogenous distribution), and large crystallites (owing to the coalescence process) [6,8,14,15,16,22]. The degree of crystallinity (DC) was determined as the ratio between the area under all diffraction peaks and the total area under the amorphous halo and diffraction peaks [14,15,16]. The intensity of the main diffraction peak of cubic spinel ferrite at (311) plane was considered as a measure of the degree of crystallinity [14,15,16].
By annealing at 500 °C, the samples α = 25, 50 and 75% display single-phase Co0.4Zn0.4Ni0.2Fe2O4, but less crystallized than the sample α = 100%, the degree of crystallinity increases with the ferrite content embedded in the SiO2 matrix. With sample α = 75% annealed at 800 °C, single phase Co0.4Zn0.4Ni0.2Fe2O4 is observed, while for sample α = 50%, the presence of trace Fe2SiO4 (JCPDS card no. 70–1861) with peaks at 2θ values of 25.04, 29.30, 31.62, 34.97, 35.91, 37.29, 41.2, 43.67, 51.39, 54.67, 55.73, 57.42, 61.17, 65.46, 68.38, 72.11, and 75.43° associated with Miller indices of (111), (002) (130), (131), (112), (200), (220), (132), (222), (061), (133), (043), (062), (162), (322), (080), and (303) is also remarked.
The formation of Fe2SiO4 appears due to the incomplete reduction of Fe3+ to Fe2+, which further reacts with the SiO2 matrix, forming Fe2SiO4 [16].
For sample α = 25% annealed at 800 °C, the main phase of Co0.4Zn0.4Ni0.2Fe2O4 is accompanied by Fe2SiO4 and quartz (JCPDS card no. 79–1910) at 2θ value of 26.6° corresponding to Miller indices of (011), whereas for sample α = 75% annealed at 1200 °C, beside the main phase of Co0.4Zn0.4Ni0.2Fe2O4, crystalline phases of SiO2 (quartz and tridymite (JCPDS card no. 042–1401)) with peaks at 2θ values of 20.76, 23.38, 27.49, 36.17, and 37.72 corresponding to Miller indices of (220), (222), (420), (040), and (240) are remarked. Unexpectedly, the samples α = 25 and 50% annealed at 1200 °C display cristobalite (JCPDS card no. 39–1425) with peaks at 2θ values of 21.98, 25.32, 28.43, 31.46, 42.66, 44.84, 47.06, 48.61, 56.22, 60.30, 62.01, 65.65, 66.81, 68.67, 69.42, 69.79, 70.54, and 72.69 associated with the Miller indices of (101), (110), (111), (102), (321), (202), (113), (212), (104), (311), (302), (204), (223), (214), (321), (303), (105), and (313) as the main crystalline phase attended by Co0.4Zn0.4Ni0.2Fe2O4 and tridymite. Additionally, for sample α = 25%, quartz is also present. The intensity of diffraction peaks belonging to the cristobalite increases with the SiO2 content.
At all annealing temperatures, for samples with no ferrite content (α = 0%), no crystalline phases are observed and the halo between 16 and 30° (2θ) matches the amorphous SiO2 matrix. A possible explanation for the absence of crystalline phases corresponding to the SiO2 could be the difficult diffusion of oxygen within the pores of the silica matrix [14,15,16]. Usually, the amorphous phase content is proportional to the area under the diffraction halo, but not all the amorphous phases produce diffraction halos due to the lack of a significant local order. The area under the amorphous halo and the total area of the diffraction peaks were used to explore the evolution of amorphous and crystalline phases [14,15,16]. Similar behavior is observed for the sample with high SiO2 matrix content (α = 25%) annealed at 500 °C. Consequently, low annealing temperature and high SiO2 content led to highly amorphous content. However, not all the amorphous phases imply diffraction halos owing to the absence of a large local order [14,21].
The average crystallite size (DXRD) was calculated using the Scherrer formula (Equation (1)):
D XRD = 0.9 · λ β · cos θ
where λ is the wavelength of CuKα radiation (1.5406 Å), β is the broadening of full width at half-maximum intensity (FWHM), and θ is the Bragg angle (°) [12,13,14,15,16].
The average crystallite size increases with the annealing temperature and Co0.4Zn0.4Ni0.2Fe2O4 content by the grain growth blocking effect of the SiO2 matrix (see Table 1) [14,15,16]. The samples with low ferrite content comprise both amorphous and crystalline phases. The changes in crystallite size may be associated with the influence of the SiO2 matrix on the grain growth and lattice strains, in such a way that SiO2 content increase, while the annealing temperature reduces the grain growth [23,24,25]. The largest crystallite size was obtained for non-embedded Co0.4Zn0.4Ni0.2Fe2O4 (α = 100%), following the assumption that the SiO2 matrix contributes to the reduction of crystallite size. One plausible explanation could be the improvement of the crystal-nuclei coalescence process, which occurs at high annealing temperatures (1200 °C). In addition, the annealing temperature reduces lattice strains and defects [14,15,16].
The lattice constant (a) was calculated using Bragg’s law with Nelson–Riley function according to Equation (2) [14,15,16]:
a = λ h 2 + k 2 + l 2 2 · sin θ
where λ is the wavelength of CuKα radiation (1.5406 Å) [15,16].
The lattice constant (a) increases with the Co0.4Zn0.4Ni0.2Fe2O4 content embedded in the SiO2 matrix and decreases with the annealing temperature (Table 1). The high surface energy and tension, surface dipole interactions, and the cation distribution inside the nanocrystallite do not produce the lattice shrinking [14,15,16,26]. The tetrahedral (A) site (0.52 Å) displays a smaller radius than the octahedral (B) site (0.81 Å) [2], while the ionic radius of Co2+ (0.75), Zn2+ (0.74,) and Ni2+ (0.69 Å) are larger than the ionic radius of Fe3+ (0.64 Å) [15]. By increasing the number of Fe3+ ions in the octahedral (B) sites, the system changes from inverse spinel to normal spinel structure [14,15,16]. Consequently, adding Co2+, Zn2+, and Ni2+ ions lead to a strained lattice.
The elemental composition is confirmed by the Co/Zn/Ni/Fe molar ratio using the MW/ICP-OES analysis (Table 1). The best experimental and theoretical data correlation is observed for the samples annealed at 1200 °C. For samples α = 25 and 50% annealed at 800 °C, the higher Fe content confirms the presence of Fe2SiO4 as a secondary phase observed by XRD.
The shape of N2 adsorption-desorption isotherms of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α (α = 0, 25, 50, 75, and 100%) samples annealed at 300 and 500 °C (Figure 4a,b) is preserved, confirming the stability of the porous structure up to 500 °C. The isotherms of samples annealed at 800 and 1200 °C could not be recorded, indicating the breakdown of porous structure at temperatures above 500 °C. The isotherm for SiO2 (α = 0%) is of type IV, and for samples α = 25, 50, and 75% is of type I [27].
The SSA decreases with the increase of α, by the increase of DXRD (Table 1). For SiO2 (α = 0%) and ferrite (α = 100%) samples, the SSA does not depend on the annealing temperature, while for samples α = 25, 50, and 75% annealed at 500 °C, an increase of SSA value was observed. A possible explanation could be the better organization and crystallization of samples annealed at 500 °C than at 300 °C. The pore size distribution (Figure 4c,d) shows that all samples contain different-sized pores up to 550 Å. The pores are generally under 100 Å in samples annealed at 500 °C and up to 200 Å in samples annealed at 300 °C, respectively. These results follow the variation of SSA described above.
The TEM image of the SiO2 matrix (α = 0%) consists of a dark area, without any possibility of identifying the matrix network, whereas those of samples α = 25–100% annealed at 500 and 800 °C are blurry, with low contrast, due to the small size poorly crystalline Co0.4Zn0.4Ni0.2Fe2O4 particles (~1 nm). For samples α = 25–100% annealed at 1200 °C (Figure 5), the higher ferrite content embedded in the SiO2 matrix results in large spherical particles. The increase in particle size from 34 to 122 nm (Table 1, Figure 6) with the ferrite content could be the outcome of different reaction kinetics, variation of the particle growth rate, or crystalline clusters formation [14,15,16,28]. The different particle arrangement could be due to the solid bodies formed by well-faceted grains, while the particle agglomeration could be a consequence of small particle size, inter-particle interactions, interfacial surface tensions, and strong intermolecular friction produced during the conversion of thermal energy into internal heat energy [14,15,16]. The porous surface formed by the gases generated during the thermal decomposition also favors the particle’s agglomeration [14,15,16].
The average crystallite sizes are consistent with the particle sizes determined from TEM, the differences being attributed to the interference in the diffraction patterns introduced by the amorphous SiO2 and large-size nanoparticles [12,13,14,15,16]. The particle size determined via TEM is generally larger than the crystallite size estimated by XRD, considering that a particle typically consists of several crystallites. The crystallite size can be calculated by analyzing the broadening of diffraction peaks without considering the effects of other factors that contribute to the diffraction peak width (i.e., instrumental contribution, temperature, microstrain, etc.) [29]. Moreover, even if they are few in number, the large nanoparticles significantly contribute to the diffraction patterns since they comprise a large fraction of atoms. The interference of the amorphous SiO2 with particle size lower than that of the embedded ferrite crystallites should also be considered [14,15,16].
The SiO2 matrix (α = 0%) displays a diamagnetic behavior (Figure 7), while samples (α = 25–100%) show a typical ferromagnetic behavior (Figure 8) both at 800 and 1200 °C.
The samples show diamagnetic behavior in the presence of some accidental low concentration of ferromagnetic impurities, which likely come from the manipulation of the samples (from cutters, tweezers, spatula, etc.). The influence of these ferromagnetic impurities on the ferrites containing samples is negligible since the magnetization of the samples reaches 10 emu/g, while the ferromagnetic impurities can provide around 0.1 emu/g.
Generally, the magnetic properties of nano-ferrites are determined by the structure, crystal defects, porosity, particle size, and K [6]. The annealing temperature and SiO2 content are critical for producing single-phase nano-ferrites with enhanced magnetic properties. The MS increases with the Co0.4Zn0.4Ni0.2Fe2O4 content and in samples with the same composition with the annealing temperature [2,6,17]. The highest value of MS (90.1 emu/g) was obtained for non-embedded Co0.4Zn0.4Ni0.2Fe2O4 (α = 100%) annealed at 1200 °C. The increase of MS from 10.0 emu/g (α = 25%) to 90.1 emu/g (α =100%) with the ferrite content is a consequence of the non-magnetic SiO2 matrix that has a magnetic dilution effect [12,13,14,15].
The nanoparticle size is contingent on the annealing temperature, which controls the formation of assemblies of weakly interacting particles through reduced magnetostatic energy and weakly bonded interfaces [14,15,16,30]. According to Neel’s theory of ferrimagnetism, the magnetic properties of ferrites depend on the distribution of magnetic ions between the tetrahedral (A) and octahedral (B) sites [2,3]. The presence of impurity atoms or oxygen vacancies results in the break of the superexchange spin coupling between magnetic ions inducing a supplementary surface spin disorder [2]. Thus, magnetization is influenced by the crystalline structure, defects, and cationic distribution. The net magnetization of these spinel structures is given by the difference between the magnetic moments of tetrahedral (A) and octahedral (B) sites [5]. Magnetization is also affected by the migration of the magnetic ions between tetrahedral (A) and octahedral (B) sites and by the magnetic moment alignment from A and B sites [5]. When the Co2+ ions occupy the octahedral (B) sites, the magnetic moment (3μB) will be higher in this position than in tetrahedral (A) sites which are occupied by Ni2+ and Zn2+ ions (2μB) [3].
The higher ferrite content in samples annealed at 1200 °C results in an MR increase from 3.3 emu/g (α = 25%) to 13.7 emu/g (α = 100%). The remanence ratio S = MR/MS indicates how square is the hysteresis loop. A theoretical value of this parameter S < 0.5 indicates samples consisting of an assembly of single domain, non-interacting particles [31,32,33]. As can be deduced from Table 2, this ratio is lower than 0.5 for all samples.
The Hc increases from 260 Oe (α = 25%) to 320 Oe (α = 100%) with ferrite content embedded in the matrix in samples annealed at 800 °C and decreases from 485 Oe (α = 25%) to 165 Oe (α = 100%) in samples annealed at 1200 °C. The samples α = 50, 75, and 100% have small Hc and high MS values due to the large particles with high magnetic coupling [31,32]. Generally, Hc depends on crystallite sizes, magnetocrystalline anisotropy, domain walls and MS [3]. In the case of small single magnetic domain particles, they change the magnetization by spin rotation [34]. At high Hc values, the thermal energy cannot induce the magnetization fluctuations for change of the magnetization [3]. Consequently, besides the particles’ shape and the density of disordered surface spins, Hc has an important contribution to the magnetic order inside a monodomain particle. For large particles, the density of surface spins is low and results in higher magnetization [26].
The magnetocrystalline anisotropy constant (K) was calculated using Equation (3):
K = μ 0 · M S · H c 2
where MS is the saturation magnetization, µ0 is vacuum permeability (μ0 = 1.256 × 10−6 N/A2), and Hc is the coercivity field (T) [35].
The K values (Table 2) increase with the Co0.4Zn0.4Ni0.2Fe2O4 content embedded in the silica matrix, with the highest K observed for the non-embedded Co0.4Zn0.4Ni0.2Fe2O4 (α = 100%). The strain on the ferrite nanoparticle surface induced by the SiO2 matrix hinders the rotation of the magnetic moments from the particle-matrix interface [32]. As can be seen from Table 2, all the main magnetic parameters were strongly affected by the SiO2 embedding. MS, MR, and K depreciate substantially with the increase of SiO2 content due to the non-magnetic nature of the matrix. The Hc value of the samples annealed at 1200 °C has a different trend; it is enhanced, suggesting the pinning of the magnetic moments from the surface of the particles, which is induced by the strain of the SiO2 layer.
The chemical composition, crystallographic structure, particle size, atomic packing density, and internal defects highly influence the ferrites’ magnetic properties [20]. Previous studies reported a decrease in the magnetocrystalline anisotropy of cubic ferrites when they are doped with Zn2+ ions [36]. Ni-Co ferrites have large K due to the Co2+ ions preference for the octahedral (B) sites [19].
The magnetization derivative curves (dM/d(µ0H)) vs. applied magnetic field are shown in the insets of Figure 8. The presence of a single peak indicates a single magnetic phase for samples α = 100%, considering that in a pure magnetic sample, the peak occurs at the nominal coercive field, suggesting crystalline samples with a single magnetic phase [14,16,31]. The sharp peaks indicate high magnetic purity, whereas the broad peaks suggest wide particle size distributions. The magnetization derivative for samples α = 25–75% annealed at 800 and 1200 °C indicate that two magnetic phases (from the triple Co–Zn–Ni ferrite) are magnetically coupled inside of the particle along their magnetic moments; the crystalline phases of Fe2SiO4 (a typical paramagnet at room temperature [34,37]), cristobalite and tridymite identified by XRD do not display magnetic properties, the hard magnetic phase being dominant (since it has a larger Hc). If not instrumental, the peaks’ asymmetry reveals the presence of two magnetic phases inside the particles, one forming from a solid solution of two ferrites and another being the third ferrite.
In our previous studies on Co–Ni, Co–Zn and Zn–Ni ferrites, only a single magnetic phase was obtained [14,15,16]. For samples annealed at 1200 °C, the hysteresis loops are, generally, broader, and the (dM/d(µ0H)) vs. µ0H curves are narrower and sharper than in samples annealed at 800 °C. The peak heights and their horizontal shifts are related to the strength of the magnetic phases [14,26,30]. For samples annealed at 800 °C, the broader peaks suggest a large particle size distribution associated with a large Hc.
The structure and the magnetic properties of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α are highly influenced by the SiO2 content and the annealing temperature. Our future studies intend to identify the metallic ion which does not couple with the other two metallic ions of the mixed ferrite leading to a second magnetic phase. Thus, by Co0.4Zn0.4Ni0.2Fe2O4 nanoparticles, the magnetic behavior can be easily tuned. Furthermore, combining the best magnetic properties and morphological configuration may be of interest for several technical applications.

4. Conclusions

The influence of SiO2 embedding on the structure, morphology, thermal, and magnetic properties of Co0.4Zn0.4Ni0.2Fe2O4 particles obtained by the sol-gel process was investigated. Fe, Co, Zn, and Ni malonates formed in two stages, as indicated on the DTA curve. At 1200 °C, the XRD and FT-IR results supported the formation of a single-phase spinel structure and SiO2 matrix. Highly crystalline single-phase ferrite starting from 300 °C for non-embedded Co0.4Zn0.4Ni0.2Fe2O4 (α = 100%) and an amorphous halo without any crystalline phases for SiO2 (α = 0%) sample were remarked. For samples α = 25–75%, the single crystalline phase Co–Ni–Zn ferrite at 500 °C was accompanied by Fe2SiO4 and quartz at 800 °C, while at 1200 °C the major cristobalite phase was accompanied by Co–Ni–Zn ferrite, tridymite, and quartz. The crystallite size increased with ferrite content in the SiO2 matrix, namely: 14.5–29.6 nm (500 °C), 26.3–52.4 nm (800 °C), and 33.3–118 nm (1200 °C), respectively. TEM images confirmed that the particles are in the nanometer range. The SSA gradually increased with the SiO2 content and decreased with the annealing temperature above 500 °C. The main magnetic parameters increased with the Co0.4Zn0.4Ni0.2Fe2O4 content: MS from 7.3 emu/g to 90.1 emu/g, MR from 1.2 to 13.7 emu/g, and K from 0.119∙10−3 to 0.934∙10−3 erg/cm3 (at 1200 °C). Hc increased with Co0.4Zn0.4Ni0.2Fe2O4 content from 260 to 320 (at 800 °C) and decreased from 485 to 165 Oe (at 1200 °C). The MS and MR increased with the annealing temperature. As expected, the non-embedded Co0.4Zn0.4Ni0.2Fe2O4 (α = 100%) was ferromagnetic with high MS, while the SiO2 matrix (α = 0%) was diamagnetic with a small ferromagnetic fraction. Co0.4Zn0.4Ni0.2Fe2O4 non-embedded into the SiO2 matrix displays the behavior of a single magnetic phase, while the Co0.4Zn0.4Ni0.2Fe2O4 embedded in the SiO2 matrix shows two magnetic phases, the solid solution of two ferrites, and the third ferrite. Moreover, when the ferrite is embedded in the SiO2 matrix, the particle sizes decreased and the main magnetic parameters depreciated.

Author Contributions

Conceptualization, T.D.; methodology, T.D., O.C. and E.A.L.; formal analysis, T.D., O.C., I.G.D., M.D.L. and E.A.L.; investigation, T.D., O.C., I.G.D., M.D.L. and E.A.L.; resources, T.D., O.C. and E.A.L.; data curation, T.D.; writing—original draft preparation, T.D., O.C., I.G.D. and E.A.L.; writing—review and editing, T.D., O.C. and E.A.L.; visualization, T.D.; supervision, T.D. All authors have read and agreed to the published version of the manuscript.

Funding

The APC was funded by the Technical University of Cluj-Napoca.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Vatsalya, V.L.S.; Sundari, G.S.; Sridhar, C.S.L.N.; Lakshmi, C.S. Evidence of superparamagnetism in nano phased copper doped nickel zinc ferrites synthesized by hydrothermal method. Optik 2021, 247, 167874. [Google Scholar] [CrossRef]
  2. Mallapur, B.M.M.; Chougule, K. Synthesis, characterization and magnetic properties of nanocrystalline Ni–Zn–Co ferrites. Mater. Lett. 2010, 64, 231–234. [Google Scholar] [CrossRef]
  3. Mohapatra, P.P.; Singh, H.K.; Kiran, M.S.R.N.; Dobbidi, P. Co substituted Ni–Zn ferrites with tunable dielectric and magnetic response for high-frequency applications. Ceram. Int. 2022, 48, 29217–29228. [Google Scholar] [CrossRef]
  4. Ghodake, J.S.; Shinde, T.J.; Patil, R.P.; Patil, S.B.; Suryavanschi, S.S. Initial permeability of Zn–Ni–Co ferrite. J. Magn. Magn. Mater. 2015, 378, 436–439. [Google Scholar] [CrossRef]
  5. Chakrabarty, S.; Bandyopadhyay, S.; Pal, M.; Dutta, A. Sol-gel derived cobalt containing Ni–Zn ferrite nanoparticles: Dielectric relaxation and enhanced magnetic property study. Mat. Chem. Phys. 2021, 259, 124193. [Google Scholar] [CrossRef]
  6. Dalal, M.; Mallick, A.; Mahapatra, A.S.; Mitra, A.; Das, A.; Das, D.; Chakrabarti, P.K. Effect of cation distribution on the magnetic and hyperfine behavior of nanocrystalline Co doped Ni–Zn ferrite (Ni0.4Zn0.4Co0.2Fe2O4). Mater. Res. 2016, 76, 389–401. [Google Scholar]
  7. Sherstyuk, D.P.; Starikov, A.Y.; Zhivulin, V.E.; Zherebstov, D.A.; Gudkova, S.A.; Perov, N.S.; Alekhina, Y.A.; Astapovich, K.A.; Vinnik, D.A.; Trukhanov, A.V. Effect of Co content on magnetic features and SPIN states in Ni–Zn spinel ferrites. Ceram. Int. 2021, 47, 12163–12169. [Google Scholar] [CrossRef]
  8. Raju, K.; Venkataiah, G.; Yoon, D.H. Effect of Zn substitution on the structural and magnetic properties of Ni–Co ferrites. Ceram. Int. 2014, 40, 9337–9344. [Google Scholar] [CrossRef]
  9. Kumar, R.; Barman, P.B.; Singh, R.R. An innovative direct non-aqueous method for the development of Co doped Ni-Zn ferrite nanoparticles. Mater. Today Commun. 2021, 27, 102238. [Google Scholar] [CrossRef]
  10. Vinnik, D.A.; Sherstyuk, D.P.; Zhivulin, V.E.; Zhivulin, D.E.; Starikov, A.Y.; Gudkova, S.A.; Zherebtsov, D.A.; Pankratov, D.A.; Alekhina, Y.A.; Perov, N.S.; et al. Impact of the Zn–Co content on structural and magnetic characteristics of the Ni spinel ferrites. Ceram. Int. 2022, 48, 18124–18133. [Google Scholar] [CrossRef]
  11. Kaur, M.; Jain, P.; Singh, M. Studies on structural and magnetic properties of ternary cobalt magnesium zinc (CMZ) Co0.6−xMgxZn0.4Fe2O4 (x = 0.0, 0.2, 0.4, 0.6) ferrite nanoparticles. Mat. Chem. Phys. 2015, 162, 332–339. [Google Scholar] [CrossRef]
  12. Stefanescu, M.; Stoia, M.; Dippong, T.; Stefanescu, O.; Barvinschi, P. Preparation of CoxFe3−xO4 oxidic system starting from metal nitrates and propanediol. Acta Chim. Slov. 2009, 56, 379–385. [Google Scholar]
  13. Shobana, M.K.; Sankar, S. Structural, thermal and magnetic properties of Ni1−xMnxFe2O4 nanoferrites. J. Magn. Mater. 2009, 321, 2125–2128. [Google Scholar] [CrossRef]
  14. Dippong, T.; Toloman, D.; Levei, E.A.; Cadar, O.; Mesaros, A. A possible formation mechanism and photocatalytic properties of CoFe2O4/PVA-SiO2 nanocomposites. Thermochim. Acta 2018, 666, 103–115. [Google Scholar]
  15. Dippong, T.; Cadar, O.; Levei, E.A.; Deac, I.G.; Borodi, G.; Barbu-Tudoran, L. Influence of polyol structure and molecular weight on the shape and properties of Ni0.5Co0.5Fe2O4 nanoparticles obtained by sol-gel synthesis. Ceram. Int. 2019, 45, 7458–7467. [Google Scholar] [CrossRef]
  16. Dippong, T.; Levei, E.A.; Cadar, O. Formation, structure and magnetic properties of MFe2O4@SiO2 (M = Co, Mn, Zn, Ni, Cu) nanocomposites. Materials 2021, 14, 1139. [Google Scholar] [CrossRef]
  17. Ramesh, S.; Sekhar, B.C.; Rao, P.S.V.S.; Rao, B.P. Microstructural and magnetic behavior of mixed Ni–Zn–Co and Ni–Zn–Mn ferrites. Ceram. Int. 2014, 40, 8729–8735. [Google Scholar] [CrossRef]
  18. Sarkar, D.; Bhattacharya, A.; Nandy, A.; Das, S. Enhanced broadband microwave reflection loss of carbon nanotube ensheathed Ni–Zn–Co-ferrite magnetic nanoparticles. Mater. Lett. 2014, 120, 259–262. [Google Scholar] [CrossRef]
  19. Stergiou, C. Magnetic, dielectric and microwave adsorption properties of rare earth doped Ni-Co and Ni-Co-Zn spinel ferrite. J. Magn. Magn. Mater. 2017, 426, 629–635. [Google Scholar] [CrossRef]
  20. Guo, H.S.; Zhang, L.; Yan, Y.L.; Zhang, J.; Wang, J.; Wang, S.Y.; Li, L.Z.; Wu, X.H. Effect of lanthanum substitution on structural, magnetic and electric properties of Ni–Zn–Co ferrites for radio frequency and microwave devices. Ceram. Int. 2022, 48, 22516–22522. [Google Scholar] [CrossRef]
  21. Wang, Y.; Gao, X.; Wu, X.; Zhang, W.; Luo, C.; Liu, P. Facile design of 3D hierarchical NiFe2O4/N-CN/ZnO composites as a high-performance electromagnetic wave absorber. Chem. Eng. J. 2019, 375, 121942. [Google Scholar] [CrossRef]
  22. Huili, H.; Grindi, B.; Viau, G.; Tahar, L.B. Influence of the stoichiometry and grain morphology on the magnetic properties of Co substituted Ni–Zn nanoferrites. Ceram. Int. 2016, 42, 17594–17604. [Google Scholar] [CrossRef]
  23. Anupama, M.K.; Rudraswamy, B.; Dhananjaya, N. Investigation on impedance response and dielectric relaxation of Ni-Zn ferrites prepared by self-combustion technique. J. Alloys Compd. 2017, 706, 554–561. [Google Scholar] [CrossRef]
  24. Amir, M.; Gungunes, H.; Baykal, A.; Almessiere, M.A.; Sozeri, H.; Ercan, I.; Sertkol, M.; Asiri, S.; Manikandan, A. Effect of annealing temperature on magnetic and Mossbauer properties of ZnFe2O4 nanoparticles by sol-gel approach. Supercond. Nov. Magn. 2018, 31, 3347–3356. [Google Scholar] [CrossRef]
  25. Asiri, S.; Sertkol, M.; Güngüneş, H.; Amir, M.; Manikandan, A.; Ercan, I.; Baykal, A. the temperature effect on magnetic properties of NiFe2O4 nanoparticles. J. Inorg. Organomet. Polym. Mater. 2018, 28, 1587–1597. [Google Scholar] [CrossRef]
  26. Ansari, S.M.; Suryawanshi, S.R.; More, M.A.; Sen, D.; Kolekar, Y.D.; Ramana, C.V. Field emission properties of nanostructured cobalt ferrite (CoFe2O4) synthesized by low-temperature chemical method. Chem. Phys. Lett. 2018, 701, 151–156. [Google Scholar] [CrossRef]
  27. Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Green Version]
  28. Bakhshi, H.; Vahdati, N.; Sedghi, A.; Mozharivskyj, Y. Comparison of the effect of nickel and cobalt cations addition on structural and magnetic properties of manganese-zinc ferrite nanoparticles. J. Magn. Magn. Mater. 2019, 474, 56–62. [Google Scholar] [CrossRef]
  29. Pussi, K.; Gallo, J.; Ohara, K.; Carbo-Argibay, E.; Kolenko, Y.V.; Berbiellini, B.; Bansil, A.; Kamali, S. Structure of Manganese Oxide Nanoparticles Extracted via Pair Distribution Functions. Condens. Mater. 2020, 5, 19. [Google Scholar] [CrossRef] [Green Version]
  30. Rao, K.S.; Choudary, G.S.V.R.K.; Rao, K.H.; Sujatha, C. Structural and magnetic properties of ultrafine CoFe2O4 nanoparticles. Proc. Mat. Sci. 2015, 10, 19–27. [Google Scholar] [CrossRef] [Green Version]
  31. Ghosh, M.P.; Mukherjee, S. Microstructural, magnetic and hyperfine characterizations of Cu-doped cobalt ferrite nanoparticles. J. Am. Chem. Soc. 2019, 102, 7509–7520. [Google Scholar] [CrossRef]
  32. Cullity, B.D.; Graham, C.D. Introduction to Magnetic Materials; John Wiley & Sons, Inc.: Hoboken, NJ, USA, 2009; 359p. [Google Scholar]
  33. Dippong, T.; Levei, E.A.; Diamandescu, L.; Bibicu, I.; Leostean, C.; Borodi, G. Structural and magnetic properties of CoxFe3−xO4 versus Co/Fe molar ratio. J. Magn. Magn. Mater. 2015, 394, 111–116. [Google Scholar] [CrossRef]
  34. Santoro, R.P.; Newnham, R.E.; Nomura, S. Magnetic properties of Mn2SiO4 and Fe2SiO4. J. Phys. Chem. Solids. 1966, 655–666. [Google Scholar] [CrossRef]
  35. Sontu, U.B.; Yelasani, V.; Musugu, V.R.R. Structural, electrical and magnetic characteristics of nickel substituted cobalt ferrite nano particles, synthesized by self combustion method. J. Magn. Magn. Mater. 2015, 374, 376–380. [Google Scholar] [CrossRef]
  36. Amer, M.A.; Tawfik, A.; Mostafa, A.G.; El-Shora, A.F.; Zaki, S.M. Spectral studies of Co substituted Ni–Zn ferrites. J. Magn. Magn. Mater. 2011, 323, 1445–1452. [Google Scholar] [CrossRef]
  37. Eibschütz, M.; Ganiel, U. Mössbauer studies of Fe2+ in paramagnetic fayalite (Fe2SiO4). Solid State Commun. 1967, 5, 267–270. [Google Scholar] [CrossRef]
Figure 1. TG (a) and DTA (b) curves of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples dried at 40 °C.
Figure 1. TG (a) and DTA (b) curves of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples dried at 40 °C.
Nanomaterials 13 00527 g001
Figure 2. FT-IR spectra of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples heated at 40 °C (a) and 300 °C (b) and XRD patterns of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples at 300 °C (c).
Figure 2. FT-IR spectra of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples heated at 40 °C (a) and 300 °C (b) and XRD patterns of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples at 300 °C (c).
Nanomaterials 13 00527 g002
Figure 3. FT-IR spectra (left) and XRD patterns (right) of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples annealed at 500, 800, and 1200 °C.
Figure 3. FT-IR spectra (left) and XRD patterns (right) of (Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α samples annealed at 500, 800, and 1200 °C.
Nanomaterials 13 00527 g003
Figure 4. N2 adsorption-desorption isotherms of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α (α = 0, 25, 50, 75, and 100%) samples annealed at 300 °C (a) and 500 °C (b) pore size distribution at 300 °C (c) and 500 °C (d).
Figure 4. N2 adsorption-desorption isotherms of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α (α = 0, 25, 50, 75, and 100%) samples annealed at 300 °C (a) and 500 °C (b) pore size distribution at 300 °C (c) and 500 °C (d).
Nanomaterials 13 00527 g004
Figure 5. TEM images of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples (α = 25–100%) annealed at 1200 °C.
Figure 5. TEM images of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples (α = 25–100%) annealed at 1200 °C.
Nanomaterials 13 00527 g005
Figure 6. Particle size distributions for (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2) 100−α samples (α = 25–100%) annealed at 1200 °C.
Figure 6. Particle size distributions for (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2) 100−α samples (α = 25–100%) annealed at 1200 °C.
Nanomaterials 13 00527 g006
Figure 7. Magnetic hysteresis loops of SiO2 matrix (α = 0%) annealed at 800 °C (a) and 1200 °C (b).
Figure 7. Magnetic hysteresis loops of SiO2 matrix (α = 0%) annealed at 800 °C (a) and 1200 °C (b).
Nanomaterials 13 00527 g007
Figure 8. Magnetic hysteresis loops and magnetization derivative of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples (α = 25–100%) annealed at 800 and 1200 °C.
Figure 8. Magnetic hysteresis loops and magnetization derivative of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples (α = 25–100%) annealed at 800 and 1200 °C.
Nanomaterials 13 00527 g008
Table 1. Particle size (DTEM), crystallites size (DXRD), crystallinity degree (DC), lattice constant (a), hopping length (LA and LB), specific surface area (SSA), and Co/Zn/Ni/Fe molar ratio of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2) 100−α samples.
Table 1. Particle size (DTEM), crystallites size (DXRD), crystallinity degree (DC), lattice constant (a), hopping length (LA and LB), specific surface area (SSA), and Co/Zn/Ni/Fe molar ratio of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2) 100−α samples.
ParameterTemp. (°C)α
0255075100
DTEM (nm)1200-34 ± 250 ± 378 ± 4120 ± 6
DXRD (nm)500-15 ± 117 ± 122 ± 130 ± 2
800-26 ± 232 ± 242 ± 351 ± 3
1200-33 ± 249 ± 375 ± 4120 ± 5
DC (%)50051 ± 359 ± 365 ± 369 ± 476 ± 5
80061 ± 366 ± 368 ± 373 ± 479 ± 4
120073 ± 481 ± 486 ± 491 ± 594 ± 5
a (Å)500-8.40 ± 0.028.41 ± 0.028.43 ± 0.028.45 ± 0.02
800-8.38 ± 0.028.39 ± 0.028.40 ± 0.028.43 ± 0.02
1200-8.36 ± 0.028.37 ± 0.028.38 ± 0.028.40 ± 0.02
SSA (m2/g)200270 ± 14220 ± 10170 ± 924 ± 119 ± 1
500260 ± 14270 ± 14260 ± 14120± 626 ± 2
800≤0.5≤0.5≤0.5≤0.5≤0.5
1200≤0.5≤0.5≤0.5≤0.5≤0.5
Co/Zn/Ni/Fe
molar ratio
500-0.37/0.38/0.19/1.970.38/0.39/0.18/1.970.39/0.38/0.17/1.980.41/0.38/0.19/2.02
800-0.31/0.29/0.18/2.200.32/0.30/0.17/2.330.39/0.38/0.18/2.030.41/0.38/0.19/2.02
1200-0.39/0.38/0.18/1.990.39/0.41/0.19/1.990.39/0.40/0.19/2.010.41/0.41/0.20/2.00
Table 2. Saturation magnetization (MS), remanent magnetization (MR), coercivity (Hc) and anisotropy constant (K) of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples annealed at 800 and 1200 °C.
Table 2. Saturation magnetization (MS), remanent magnetization (MR), coercivity (Hc) and anisotropy constant (K) of (Co0.4Zn0.4Ni0.2Fe2O4)α(SiO2)100−α samples annealed at 800 and 1200 °C.
Sample
(Co0.4Zn0.4Ni0.2Fe2O4)α (SiO2)100−α
Temperature
(°C)
Ms
(emu/g)
MR
(emu/g)
SHc
(Oe)
K·105
(erg/cm3)
α = 25%8007 ± 0.41.2 ± 0.10.17 ± 0.02260 ± 13119 ± 6
120010 ± 13.3 ± 0.20.33 ± 0.03490 ± 25305 ± 15
α = 50%80014 ± 12.6 ± 0.10.19 ± 0.02270 ± 14229 ± 11
120029 ± 25.3 ± 0.30.18 ± 0.02320 ± 16577 ± 29
α = 75%80023 ± 15.7 ± 0.30.25 ± 0.03300 ± 15437 ± 22
120062 ± 49.8 ± 0.50.16 ± 0.02220 ± 11857 ± 43
α = 100%80038 ± 28.7 ± 0.40.23 ± 0.02320 ± 16754 ± 38
120090 ± 614 ± 10.15 ± 0.02170 ± 10934 ± 47
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Dippong, T.; Levei, E.A.; Deac, I.G.; Lazar, M.D.; Cadar, O. Influence of SiO2 Embedding on the Structure, Morphology, Thermal, and Magnetic Properties of Co0.4Zn0.4Ni0.2Fe2O4 Particles. Nanomaterials 2023, 13, 527. https://doi.org/10.3390/nano13030527

AMA Style

Dippong T, Levei EA, Deac IG, Lazar MD, Cadar O. Influence of SiO2 Embedding on the Structure, Morphology, Thermal, and Magnetic Properties of Co0.4Zn0.4Ni0.2Fe2O4 Particles. Nanomaterials. 2023; 13(3):527. https://doi.org/10.3390/nano13030527

Chicago/Turabian Style

Dippong, Thomas, Erika Andrea Levei, Iosif Grigore Deac, Mihaela Diana Lazar, and Oana Cadar. 2023. "Influence of SiO2 Embedding on the Structure, Morphology, Thermal, and Magnetic Properties of Co0.4Zn0.4Ni0.2Fe2O4 Particles" Nanomaterials 13, no. 3: 527. https://doi.org/10.3390/nano13030527

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.