Mineral Composition and Graphitization Structure Characteristics of Contact Thermally Altered Coal

1
College of Safety Science and Engineering, Anhui University of Science and Technology, Huainan 232000, China
2
State Key Lab of Coal Mine Safety Technology, Shenyang Research Institute, China Coal Technology and Engineering Group, Fushun 113122, China
3
Exploration Research Institute, Anhui Provincial Bureau of Coal Geology, Hefei 230088, China
4
Key Laboratory of Intelligent Underground Detection Technology, School of Civil Engineering, Anhui Jianzhu University, Hefei 230601, China
5
School of Architecture & Urban Planning, Anhui Jianzhu University, Hefei 230601, China
*
Authors to whom correspondence should be addressed.
Molecules 2022, 27(12), 3810; https://doi.org/10.3390/molecules27123810
Submission received: 23 March 2022 / Revised: 28 May 2022 / Accepted: 2 June 2022 / Published: 14 June 2022
(This article belongs to the Section Molecular Structure)

Abstract

:
Contact metamorphism in coal is usually characterized by a rapid, brief, and exotherm reaction that can change the geothermal gradient. In this process, coal adjacent to the intrusive body can form thermally altered coal-based graphite (TACG). In order to further study the structural changes of TACG at different distances from the intrusive body, four TACG samples were collected in the Zhuji coal mine in the Huainan Coalfield, North China, and their vitrinite reflectance and Raman spectra were measured using polarizing microscopy and Raman spectroscopy. The results showed that: (1) affected by the temperature and stress of magmatic hydrothermal intrusion, the clay minerals in the coal seams appeared distributed in strips; the occurrence of ankerite and pyrite in the coal seams near the magmatic intrusions could be due to a late magmatic hydrothermal mineralization; (2) the Rmax − Rmin correlation for the TACG samples under study showed that thermal metamorphism was the main factor leading to the graphitization of the TACG samples, without an obvious pressure effect; (3) with the increase of the graphitization process, the D- and G-band showed some similar changes, specifically, their peak positions shifted to lower wave numbers, and the full width at half maximum (FWG and FWD) gradually decreased; the difference was that the intensity of the G-band increased, while that of the D-band decreased; (4) the graphitization degree of the TACG samples increased with the increase of the transverse size of the crystals, while the FWG and FWD values of the G- and D-band decreased; (5) in comparison to natural graphite, the TACG still presented structural defects.

1. Introduction

Carbonaceous materials (CM) have attracted research interest worldwide in recent years. In the process of geological evolution, CM in nature can be gradually transformed into disordered graphite. With the continuous improvement of the order degree, ordered graphite can form [1,2].
Thermal events related to igneous intrusion are relatively common in many countries in the world, and a large number of studies have been conducted on the impact of igneous intrusion on coal [3,4,5,6,7,8,9,10,11,12,13,14,15,16,17]. Especially, research has been carried out on some representative coalfields i.e., the Illinois, Raton and San Juan Basins in the USA, the Gunnedah Basin and Bowen Basin in Australia, and the Qinshui, Fushun and Tiefa Basins in China [6,8,10,11,18,19,20,21]. In these coalfields, some coal seams and their surrounding rocks were invaded by dikes, sills, and other types of igneous rocks. The heat generated by this invasion may be as high as 600 °C, or even higher during invasion, causing significant changes in the coal. More generally, the higher the temperature, the more obvious the changes are. Therefore, it is possible to trace the changes in the structure of coal at different distances from the intrusive body.
More generally, these effects of heat are local and variable and, geologically speaking, they occur over a comparatively short period. This kind of alteration contrasts with the normal progression of coal rank which is a regional and slow process in response to normal, rather than abnormal, upper crustal temperatures [22]. Compared with coal during normal coalification, thermally altered coal has typical physicochemical characteristics [10,11,13,19,20]. For example, the vitrinite reflectance of coal increases, but the moisture, volatile matter, and hydrogen content decrease as the distance from the intrusion decreases. Significantly, when coal is transformed into graphite by contact thermal metamorphism, the resulting graphite can be called thermally altered coal-based graphite (TACG) [23].
The technical methods commonly used in TACG research are usually two: optical microscopy (high-resolution electron microscopy (HREM)) and spectroscopy (X-ray diffraction (XRD) and Raman spectroscopy). HREM was used to study coal-based graphite series samples. The results showed that the transition from coal to graphite formed a two-dimensional graphite lattice (aromatic graphite) in the first stage, then three-dimensional lattice graphite microcrystals (microcolumn graphite and soft graphite), and finally flat graphite [24]. In the transformation from amorphous to crystalline, the basic process was the lateral expansion of the two-dimensional graphite carbon layer and the increase of the thickness of the graphite carbon layer. If the graphite carbon layer was regarded as a complete lattice region, then the random carbon atom region between the graphite carbon layers was the “Defect” region of the coal structure. This “Defect” region was called the original structural defect in the graphitization process of coal. Therefore, the whole graphitization process was the process of reducing the “Defect” region of the original structure until it was finally eliminated. Because of the advantage of causing minimum damage to CM chemical structure, XRD can effectively study the crystal structure characteristics of CM [24]. Five structural parameters, including amorphous carbon fraction (A), aromaticity (fa), interlayer spacing of the crystal structure (d002), and crystallite size (La and Lc), are commonly used to define the carbon stacking structure of CM [25]. The Raman spectra of CM are usually divided into first-order and second-order regions [26]. The first-order region, especially the graphite zone (G) and the defect zone (D) at 1582 and 1357 cm−1, respectively, reflects the structural order of the CM [27,28,29,30]. For perfect single graphite crystals, the G-band becomes visible at 1580 cm−1, accompanied by a strong C-C stretching mode (E2g2 vibration mode), which indicates the stretching vibration of sp2 bonds in hexagonal aromatic molecules. On the contrary, for disordered structural CM, the D-band (in-plane defect), which represents the graphite lattice vibration and has A1g symmetry, appears. The disorder degree of carbon structure in CM can be distinguished by comparing the D- and the G-band in Raman spectra [31].
For TACG, previous research mainly focused on the characterization of coal-based graphite, the integrity of coal crystals, and the ordering of coal structures. There is still a lack of in-depth research on whether the “Defect” region of TACG is caused by original structural defects or by secondary structural defects. Therefore, in this study, TACG samples with different distances from the intrusion were collected, and the vitrinite reflectance and Raman spectra of these samples were obtained by polarizing microscopy and laser Raman spectroscopy. By means of a comparative study and a graphic method, we discuss in depth whether the TACG samples were affected by intrusion pressure and the attribution of the “Defect” region of these samples.

2. Geological Backgrounds

The Huainan Coalfield is located in northern Anhui Province at the southeast corner of the North China Plate (Figure 1a). It is an elongated territory with a mean length of 180 km (W-E) and a width of 15–25 km (N-S). During the Yanshan period, magma intruded extensively into the early Permian coal-bearing strata. Magmatic activities in this period mainly intruded into coal measures through some small and medium-sized dikes and sills, which affected the coal seams in the mine field. Igneous intrusion takes various forms, including intrusion along the coal seam roof, direct cut into the coal seam, and intrusion along the coal seam floor [23]. The Zhuji coal mine is located in the northeast of the Huainan coalfield, with an area of 54.13 km2, and its coal reserves are about 950 million tons (Figure 1a). The geological structure of Zhuji coal mine mainly consists of broad shallow dip folds and sporadic faults. The Permian coal-bearing strata in Zhuji coal mine is divided into Shanxi formation, lower Shihezi formation, and upper Shihezi formation. Detailed information on the location and thickness of each coal seam is documented in Figure 1b. Igneous intrusion in Zhuji coal mine is very obvious. Magma intruding into coal-bearing strata ranges from exploration line 6 in the east to exploration line 15 in the west. In addition, the location of igneous intrusion gradually rises from the east No. 3 coal seam to the west No. 8 coal seam. In recent years, the main coal seam mined in Zhuji coal mine was the No. 4 coal seam, located in the east of the mining area. In Figure 1c, the No. 4 coal seam appears obviously affected by igneous intrusion.

3. Samples and Experiments

3.1. Sampling

Figure 1c shows the position information of four TACG samples at different distances from the intrusion. These samples were collected from the underground working faces of the No. 4 coal seam, and the sampling method used was channeling sampling. After carefully identifying the contact zone between the intrusion and the coal seam, fresh TACG samples were collected, and the gangue was removed.

3.2. Coal Quality

In this study, Rmax (maximum reflectance), Rmin (minimum reflectance), and Ro (mean reflectance) of TACG samples were determined according to GB/T6948-2008. All reflectance values were measured using an optical microscope (Leica DM 6000 M) at a 546 nm wavelength in oil immersion. A resolution of 50/0.85 was used for oil-immersed objects. The test results are listed in Table 1.
In addition, the proximate analysis indexes of coal were measured, including ash content (Ad, %), volatile matter (Vdaf, %), and moisture (Mad, %). These indexes are helpful to analyze and understand the metamorphic degree of coal. As can be seen in Table 1, the ash content of the four coal samples in the study area was between 17.05–19.69%, and the volatile content was between 8.06–8.91%, values typical of low-middle ash coal and low volatile coal. The organic macerals in coal were mainly vitrinite, followed by inertinite and crustite. The inorganic components in coal were mainly clay minerals, followed by carbonate minerals, with scattered sulfides (Figure 2). In addition, it can be seen in Figure 2 that the four coal samples in the study area were affected by magma intrusion, and the coal petrographic components in the coal were often flattened, with a certain directionality, curved cracks, and obvious rheological phenomena (Figure 2c,d).

3.3. Field Emission Scanning Electron Microscopy

Pretreatment of the TACG samples and experiments were carried out in the State Key Laboratory of Solid Microstructure Physics, School of Physics, Nanjing University. Sample pretreatment adopted the argon ion polishing sample preparation method. The model of the polishing machine was TIC 3X, and three ion guns were used for plane polishing. Three-beam plane polishing was used, and the surface of the sample was superfinished in a vacuum environment to remove scratches, particles, organic pollutants, and stress damage layers; a flat and crystalline sample surface was obtained for observation of its nanoscale structures. The polishing setting was voltage of 5.0 kV, current of 2.0 mA, and polishing time of 2 h. The polished sample was observed under the ultra-high resolution scanning electron microscope Gemini-SEM 500, and the voltage was set at 2.0 kV. A field emission scanning electron microscope (FESEM) was used to observe the thermal simulation series of coal samples after argon ion polishing treatment, and the pore and mineral distribution characteristics of four metamorphic series of coal samples were analyzed.

3.4. Raman Spectroscopy

Raman measurement of the TACG samples were performed with a Raman Spectroscope (Bruker Corporation) equipped with an Nd-YAG laser as an excitation light source. A laser beam of 532 nm was focalized onto the TACG samples to collect the Raman signals in backscattered direction. The laser power was set at 1 mW. The diameter of the laser spot on each analytical sample was 1 μm. Samples with a diameter <56 μm were scanned between 800 cm−1 and 2000 cm−1, covering the first-order region. The average acquisition time for each spectrum was 45 s.

4. Results and Discussion

4.1. Organic Matter and Mineral Characteristics

Figure 3 shows a scanning electron microscope photograph of a coal sample. As can be seen, the pores in the coal had various shapes, round and oval, often formed by the dissolution of heated liquid, with burrs and harbor shapes. The pore size of the heat altered pores ranged from <0.1 μm to >10 μm (Figure 3a). It is generally believed that the formation of thermal porosity is related to the generation and escape of volatiles when coal is softened by heat. Radial cracks and sometimes annular cracks are common in the walls and peripheries of some heat-changing pores, and their causes are related to the shrinkage caused by the escape of volatiles in thermoplastic state (Figure 3b,c). We observed globules sprouting around the hot pores and at the bottom of the pores. The particle size and anisotropy of the globules around the pores increased towards the center of the pores. Some pores were filled with hydrothermal minerals such as quartz and calcite, which indicated that the inner walls of these pores had been in contact with the heat-carrying fluid, and the heat energy brought by the heat-carrying fluid caused mesophase globules to sprout from vitrinite (Figure 3d).
Figure 4 shows a scanning electron micrograph of organic matter pores and the mineral composition of the samples in the study area. It can be seen that the structure of the immature intact coal was relatively compact, with few mineral intragranular pores and intergranular pores with organic matter, and only a small number of organic pores were developed, mainly in the shape of ellipses and long strips. Most of the organic pores were of micron size, with a small number of nano-sized pores, and pore sizes fluctuated within the range from 100 nm to 600 nm (Figure 4a). Because coal samples were in a lowly mature state, the pores and fissures in the coal were formed by the compression and dehydration shrinkage of the plant primary pores and the coal by external forces, and micro-nano pores did not developed in the vitrinite. As the distance from the igneous intrusion decreased, the thermal magmatism of the coal increased, and the nano-scale pores in the coal increased, mainly in the form of long strips and ellipses, with pore sizes ranging from 100 to 300 nm. the pore walls were round and smooth and accompanied by a small number of micro-fissures. The micro-fissures were often connected with the nano-scale pores, so that the connectivity of the pores was better (Figure 4b). When the distance was about 10 cm from the igneous intrusion, the pore walls of the fissures in the organic material were rough, which might be caused by the high pressure generated by high-temperature condensation polymerization, which generated coal fissures (Figure 4c).
In addition, the intrusion of the magmatic hydrothermal solution changed the coal in the contact zone with the coal seam into high-rank metamorphic coal and natural coke. The minerals in coal were mainly quartz and kaolinite. At the same time, calcite, pyrite, and other minerals were in contact with the coal seam along the hydrothermal channel of magma, resulting in different mineral compositions in adjacent coals. Therefore, the local distance between samples and magmatic rocks could be inferred from the mineral composition. As can be seen in Figure 4e, the clay minerals in the coal seam were distributed in a strip shape under the influence of temperature and stress caused by magmatic hydrothermal intrusion. The occurrence of ankerite and pyrite in the coal seams close to the magmatic intrusions could be due to late magmatic hydrothermal mineralization (Figure 4f).

4.2. Effect of Pressure

Through a study of the reflectance of coal carbonized in the laboratory without excess pressure and under pressure, Chandra [32] proposed that the effect of pressure on TACG could be obtained by measuring the Rmax and Rmin of vitrinite. If the reflectance characteristics of TACG are similar to those of residues of coals carbonized in the laboratory without excess pressure, then the pressure effect can be considered negligible or non-existent. If the reflectance characteristics of TACG are different from those of the residues of coals carbonized in the laboratory without excess pressure, the difference indicates the effect of pressure on TACG.
On the basis of the experimental results of Chandra (1965), the Rmax and Rmin of TACG were represented in a Rmax − Rmin diagram, and the following conclusions were drawn by comparing the Rmax − Rmin relationship with that of other TACG (Figure 5). We found that: (1) the Rmax-Rmin relationship of TACG was similar to that of Wilsontown Main coals (Riddochhill colliery, East Ayrshire, Scotland), and the values of Rmax and Rmin for the studied TACG and Wilsontown Main coals were similar to those for coals (85% and 98% carbon content) carbonized in the laboratory without excess pressure. In particular, the Rmax − Rmin relationship of TACG was highly consistent with that of 89% carbonized coal. It can be reasonably concluded that the effect of pressure, if any, during thermal metamorphism, on the studied TACG and Wilson town Main coals can be neglected; (2) the results of High Coal Sill coals and Antarctic coals were different from those of coals carbonized in the laboratory without pressure. The Rmax − Rmin relationship of the above two coals showed a higher degree of anisotropy than that found in the carbonization test of the full-order series of coals without overpressure in the laboratory. Consequently, these two coals might be subject to overpressure during thermal metamorphism. This conclusion is supported by the observation results of carbonized coal under laboratory pressure.
More generally, there are many forms of igneous intrusion into coal-series strata, which were summarized by Yao and Liu [11]. They concluded that if the magma intrudes along the roof of the coal seam, it releases a large amount of heat to the lower coal seam, causing thermal deterioration of the coal; if the magma is obliquely inserted into the coal seam, brittle deformation of coal occurs due to the existence of a certain “wedge stress”. The Rmax–Rmin relationship of TACG in this study showed that there was no obvious pressure effect, so it can also be suggested that the magma would intrude along the roof of the coal seam, which is consistent with the actual observation results.

4.3. Raman Spectra

The first-order Raman spectra of the four graphitized series samples ZJ1, ZJ2, ZJ3, and ZJ4 are presented in Figure 6a. In this paper, three Raman parameters proposed by Tuinstra and Koenig [33] for CM were used: (1) Raman shift frequencies of the wE2g spectral peak (G-band) and wA1g spectral peak (D-band); the diffraction peaks of each sample were mainly the G and D peaks; (2) FWG of the E2g spectral peak and FWD of the A1g spectral peak; (3) the ratio of the peak intensity of the A1g spectral peak to the peak intensity of the E2g spectral peak (ID/IG). According to this, after the noise on the experimental spectrogram was removed and using the Fit Multi-peaks function (Lorentzian) in Origin 2017 software, the main Raman parameters of each sample were respectively obtained, as shown in Table 2.
Through spectrum fitting (Figure 6b), it was found that two peaks were fitted in the D-band, namely, the D peak (1320 cm−1) caused by C–C bond vibration between aromatic ring and aromatic compound with not less than six rings, and the Ds peak (1360 cm−1) [29], which was the sub-peak of the D peak and mainly derived from the stretching vibration of amorphous carbon structure. Similarly, two peaks were fitted in the G-band, namely, the G peak (1580 cm−1), caused by the aromatic ring stretching vibration and the alkene C=C bond vibration [28], and the Gs peak (1600 cm−1), which was the sub-peak of the G peak [29]. In the following analysis, for convenience of expression, the A1g peak (D-band) corresponds to the fitted D peak, and the E2g peak (G-band) corresponds to the fitted G peak [30]. The above-mentioned shift frequencies, FWHM, and peak intensity ratios were all obtained from the fitted D- and G-peak.
A group of coal-based graphite samples with different graphitization degrees are shown in Figure 6a. As mentioned earlier [27,34,35], the 1580 cm−1 spectral peak of this spectrogram was a two-dimensional lattice stretching vibration peak, which is the natural spectral peak (G peak) of graphite. Obviously, the G peak is relatively stable, its intensity increases with the improvement of the coal-based graphite lattice, and its peak shape is sharp. This was clearly shown by the spectral peaks of the samples shown in Figure 6a. Compared with other samples, the ZJ4 sample had a low graphitization degree, accompanied by low G peak intensity and narrow G peak width (FWG = 29 cm−1), which means that its lattice integrity was not high. With the increase of the graphitization degree, the G peak of the ZJ-3, ZJ2, and ZJ1 sequence samples became higher and sharper, and the corresponding FWG decreased from 27 cm−1 to 20 cm−1.
According to the calculation and analysis by [33], the spectrum peak near 1320 cm−1 was the A1g peak, which was caused by structural defects. As can be seen in Figure 6b, the intensity of the D peak near 1320 cm−1 gradually weakened with the increase of the graphitization degree and gradually became a secondary spectral peak compared with the G peak. Therefore, the decrease of the spectral peak near 1320 cm−1 indicated that the structural defects of the peak steadily disappeared and were replaced by the integrated lattice region during the graphitization process. Therefore, the structural defects reflected by this spectral peak had the characteristics of primary structural defects.

4.4. Relationship between La and FWG and FWD

Tuinstra and Koenig [33] considered that the A1g spectrum peak was the carbon layer diameter effect of graphite crystallites. Due to the small crystallite size, the A1g vibration turned into Raman activity, and the 1320 cm−1 spectrum peak (D peak) was generated. From this, the intensity of the D peak is proportional to the diameter La of the crystallite carbon layer
L a = 44 / ( I D I G )
where the unit of La is Å (10−1 nm), and ID and IG are the intensities of D- and G-peak, respectively. According to this formula, the Raman spectrum data of each sample listed in Table 2 were used to obtain the corresponding La values, which are listed in the right end of Table 2.
The La-FWD and La-FWG diagrams are shown in Figure 6a,b. In Figure 6, it can be observed that the graphitization process increased with the increase of La, but FWG and FWD decreased gradually, as shown in the graphitization process curve in (Figure 7).
Vibration analysis showed [36,37] that the factor group analysis of the integrated graphite lattice space group is the basis for understanding the Raman spectra of graphitized CM. Graphite cells have four carbon atoms, which has nine vibration modes, described as:
2 B 1 g ( ) + 2 E 2 g ( R ) + A 2 g ( I R ) + E 1 u ( I R )
where ( ) is infrared and Raman inactivity; (R) is Raman activity; (IR) is infrared activity.
For other graphite materials that are not single crystals, only one layer of carbon atoms needs to be analyzed, because the vibrational coupling between the graphite carbon layers is very weak and can be omitted. Therefore, graphite is considered a two-dimensional lattice with two carbon atoms in the cell, and its two vibrational modes can be described as:
B 1 ( ) + E 2 g ( R )
Therefore, the two-dimensional lattice graphite has only one E2g vibration mode. In this mode, the reciprocal points within a layer of carbon atoms and on its boundaries are possible vibrational phonons. For ideal graphite lattice, the vibration phonon symmetry is high, and its vibration frequency can be cancelled or strengthened. Therefore, the phonon vibration on the graphite carbon layer cannot cause a change in polarization, exhibiting non-Raman activity (only the G peak vibration). That is, as the diameter of the carbon layer (La) increases gradually, the higher the symmetry of the vibration phonons on the carbon layer, the lower the polarization caused by the vibration, the higher the intensity of the G peak, and the lower the FWG value. This is consistent with Figure 6a. The regression equation between La and FWG of coal-based graphite sequence samples was obtained in this study:
L a = 0.09948 FW G + 35.02849   ( Correlation   coefficient   r = 0.84 )
Similarly, for finite-size graphite crystallites, the A1g mode will change to Raman activity, and the D peak vibration caused by the boundary defects of graphite carbon layer will be strengthened. That is, as the diameter of the carbon layer (La) increases gradually, the mode A1g will change to non-Raman activity, the vibration effect of D peak will decrease, and its intensity and FWD value will also decrease. This is consistent with Figure 6b. The regression equation between La and FWD of the coal-based graphite sequence samples was obtained in this study:
L a = 0.13135 FW D + 48.99568   ( Correlation   coefficient   r = 0.95 ) .
In accordance with the Raman spectrum characteristics of coal-based graphite, the D band of graphite can be divided into two types of structural defect bands with different properties [33]. One is the original structure defect band; the other is the secondary structure defect band. According to Nakamizo et al. [37], the latter is usually caused by shear pressure or grinding. On this basis, combined with Figure 6, it can be concluded that the D peak of the studied TACG samples could be caused by its original structural defects.

5. Conclusions

The main conclusions of this study are as follows: (1) affected by the temperature and stress of igneous intrusion, the clay minerals in the coal seams were distributed in strips. The occurrence of ankerite and pyrite in the coal seams near the magmatic intrusions could be due to late magmatic hydrothermal mineralization; (2) The Rmax–Rmin correlation confirmed that four TACG were not subjected to obvious magmatic shear pressure; (3) with the increase of the graphitization process, the positions of the D- and G-peak shifted to a lower wavenumber. The intensity of the G peak increased, and the spectral pattern was sharp, while the intensity of the D peak decreased, and the spectral pattern was low. The FWHM values of the D- and G-peak decreased; (4) the FWHM of the D- and G-peak showed a significant positive correlation with La, indicating that with the intensification of the graphitization process, the degree of the lattice defects in coal-based graphite decreased, and the crystal form tended to be integrated.

Author Contributions

Conceptualization and writing—original draft preparation, H.L.; Methodology, W.L. and G.H.; Investigation, C.W.; Software, X.G.; Writing—review and editing, D.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the general Project of Natural Science Foundation of Anhui Province (2018A040106), the Key Research and Development Projects in Anhui Province (201904a07020071).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

Sample Availability

Coal samples are not available from the authors.

References

  1. Ferrari, A. Raman spectroscopy of graphene and graphite: Disorder, electron–phonon coupling, doping and nonadiabatic effects. Solid State Commun. 2007, 143, 47–57. [Google Scholar] [CrossRef]
  2. Slonczewski, J.; Weiss, P. Band structure of graphite. J. Chem. Phys. 2008, 21, 2238–2239. [Google Scholar] [CrossRef]
  3. Clegg, K. Metamorphism of Coal by Peridotite Dikes in Southern Illinois. In State Geological Survey Report of Investigations; Geological Survey Library: Urbana, IL, USA, 1955; Volume 178, pp. 17–18. [Google Scholar]
  4. Johnson, R. Coal Resources of the Trinidad Coal Field in Huerfano and Las Animas Counties, Colorado: A Resume of the Coal Resources in an Area of 1100 Square Miles in South-Central Colorado. No. 1112; US Government Printing Office: Washington, DC, USA, 1961.
  5. Meyers, P.; Simoneit, B. Effects of extreme heating on the elemental and isotopic compositions of an Upper Cretaceous coal. Org. Geochem. 1999, 30, 299–305. [Google Scholar] [CrossRef]
  6. Gurba, L.; Weber, C. Effects of igneous intrusions on coalbed methane potential, Gunnedah Basin, Australia. Int. J. Coal Geol. 2001, 46, 113–131. [Google Scholar] [CrossRef]
  7. Stewart, A.; Massey, M.; Padgett, P.; Rimmer, S.; Hower, J. Influence of a basic intrusion on the vitrinite reflectance and chemistry of the Springfield (No. 5) coal, Harrisburg, Illinois. Int. J. Coal Geol. 2005, 63, 58–67. [Google Scholar] [CrossRef]
  8. Cooper, J.; Crelling, J.; Rimmer, S.; Whittington, A. Coal metamorphism by igneous intrusion in the Raton Basin, CO and NM: Implications for generation of volatiles. Int. J. Coal Geol. 2007, 71, 15–27. [Google Scholar] [CrossRef]
  9. Saghafi, A.; Pinetown, K.; Grobler, P.; Vanheerden, J. CO2 storage potential of South African coals and gas entrapment enhancement due to igneous intrusions. Int. J. Coal Geol. 2008, 73, 74–87. [Google Scholar] [CrossRef]
  10. Rimmer, S.; Yoksoulian, L.; Hower, J. Anatomy of an intruded coal, I: Effect of contact metamorphism on whole-coal geochemistry, Springfield (No. 5) (Pennsylvanian) coal, Illinois Basin. Int. J. Coal Geol. 2009, 79, 74–82. [Google Scholar] [CrossRef]
  11. Yao, Y.; Liu, D. Effects of igneous intrusions on coal petrology, pore-fracture and coalbed methane characteristics in Hongyang, Handan and Huaibei coalfields, North China. Int. J. Coal Geol. 2012, 96–97, 72–81. [Google Scholar] [CrossRef]
  12. O’Keefe, J.; Bechtel, A.; Christanis, K.; Dai, S.; DiMichele, W.; Eble, C.; Esterle, J.; Mastalerz, M.; Raymond, A.; Valentim, B.; et al. On the fundamental difference between coal rank and coal type. Int. J. Coal Geol. 2013, 118, 58–87. [Google Scholar] [CrossRef]
  13. Xu, C.; Cheng, Y.; Wang, L.; Zhou, H. Experiments on the effects of igneous sills on the physical properties of coal and gas occurrence. J. Nat. Gas Sci. Eng. 2014, 19, 98–104. [Google Scholar] [CrossRef]
  14. Rahman, M.; Rimmer, S. Effects of rapid thermal alteration on coal: Geochemical and petrographic signatures in the Springfield (No. 5) Coal, Illinois Basin. Int. J. Coal Geol. 2014, 131, 214–226. [Google Scholar] [CrossRef]
  15. Aghaei, H.; Gurba, L.; Ward, C.; Hall, M.; Mahmud, S. Effects of igneous intrusions on thermal maturity of carbonaceous fluvial sediments: A case study of the Early Cretaceous Strzelecki Group in west Gippsland, Victoria, Australia. Int. J. Coal Geol. 2015, 152, 68–77. [Google Scholar] [CrossRef]
  16. Jiang, J.; Zhang, Q.; Cheng, Y.; Jin, K.; Zhao, W.; Guo, H. Influence of thermal metamorphism on CBM reservoir characteristics of low-rank bituminous coal. J. Nat. Gas Sci. Eng. 2016, 36, 916–930. [Google Scholar] [CrossRef]
  17. Jiang, J.; Zhang, Q.; Cheng, Y.; Wang, H.; Liu, Z. Quantitative investigation on the structural characteristics of thermally metamorphosed coal: Evidence from multi-spectral analysis technology. Environ. Earth Sci. 2017, 76, 406. [Google Scholar] [CrossRef]
  18. Glikson, M.; Boreham, C.; Thiede, D. Coal Composition and Mode of Maturation, a Determining Factor in the Quantifying Hydrocarbon Species Generated. In Coalbed Methane: Scientific, Environmental and Economic Evaluation; Mastalerz, M., Glikson, M., Golding, S.Ž., Eds.; Kluwer Academic Publishers: Dortrecht, The Netherlands, 1999; pp. 155–185. [Google Scholar]
  19. Golab, A.; Carr, P. Changes in geochemistry and mineralogy of thermally altered coal, Upper Hunter Valley, Australia. Int. J. Coal Geol. 2004, 57, 197–210. [Google Scholar] [CrossRef]
  20. Pratheesh, P.; Prasannakumar, V.; Prasannakumar, K. Praveen Geochemistry of the late phanerozoic mafic dykes from the Moyar shear zone, South India, and its implications on the spatial extent of Deccan Large Igneous Province. Arab. J. Geosci. 2013, 6, 3281–3291. [Google Scholar] [CrossRef]
  21. Jiang, J.; Cheng, Y.; Zhang, P.; Jin, K.; Cui, J.; Du, H. CBM drainage engineering challenges and the technology of mining protective coal seam in the Dalong Mine, Tiefa Basin, China. J. Nat. Gas Sci. Eng. 2015, 24, 412–424. [Google Scholar] [CrossRef]
  22. Kisch, H.; Taylor, G. Metamorphism and alteration near an intrusive-coal contact. Econ. Geol. 1966, 61, 343–361. [Google Scholar] [CrossRef]
  23. Bostick, N.; Collins, B.; Bostick, N. Petrography and programmed pyrolysis of coal and natural coke intruded by an igneous dike, Coal Basin, Pitkin County. Teach. Geogr. 1987, 22, 92–93. [Google Scholar]
  24. Lu, L.; Sahajwalla, V.; Kong, C.; Harris, D. Quantitative X-ray diffraction analysis and its application to various coals. Carbon 2001, 39, 1821–1833. [Google Scholar] [CrossRef]
  25. Iwashita, N.; Inagaki, M. Relations between structural parameters obtained by X-ray powder diffraction of various carbon materials. Carbon 1993, 31, 1107–1113. [Google Scholar] [CrossRef]
  26. Wu, D.; Liu, G.; Sun, R.; Fan, X. Investigation of Structural Characteristics of Thermally Metamorphosed Coal by FTIR Spectroscopy and X-ray Diffraction. Energy Fuels 2013, 27, 5823–5830. [Google Scholar]
  27. Cuesta, A.; Dhamelincourt, P.; Laureyns, J.; Martinez-Alonso, A.; Tascón, J. Raman microprobe studies on carbon materials. Carbon 1994, 32, 1523–1532. [Google Scholar] [CrossRef]
  28. Jawhari, T.; Roid, A.; Casado, J. Raman spectroscopic characterization of some commercially available carbon black materials. Carbon 1995, 33, 1561–1565. [Google Scholar] [CrossRef]
  29. Mennella, V.; Monaco, G.; Colangeli, L.; Bussoletti, E. Raman spectra of carbon-based materials excited at 1064 nm. Carbon 1995, 33, 115–121. [Google Scholar] [CrossRef]
  30. Ferrari, A.; Robertson, J. Interpretation of Raman spectra of disordered and amorphous carbon. Phys. Rev. B 2000, 61, 14095–14107. [Google Scholar] [CrossRef] [Green Version]
  31. Zerda, T.; John, A.; Chmura, K. Raman studies of coals. Fuel 1981, 60, 375–378. [Google Scholar] [CrossRef]
  32. Chandra, D. Use of reflectance in evaluating temperature of carbonized or thermally metamorphosed coals. Fuel 1965, 44, 171–176. [Google Scholar]
  33. Tuinstra, F.; Koenig, J. Raman spectrum of graphite. J. Chem. Phys. 1970, 53, 1126–1130. [Google Scholar] [CrossRef] [Green Version]
  34. Hiura, H.; Ebbesen, T.; Tanigaki, K.; Takahashi, H. Raman studies of carbon nanotubes. Chem. Phys. Lett. 1993, 202, 509–512. [Google Scholar] [CrossRef]
  35. Sonibare, O.; Haeger, T.; Foley, S. Structural characterization of Nigerian coals by X-ray diffraction, Raman and FTIR spectroscopy. Energy 2010, 35, 5347–5353. [Google Scholar] [CrossRef]
  36. Hirsch, P. X-ray Scattering from Coals. Proc. R. Soc. A 1954, 226, 143–169. [Google Scholar]
  37. Nakamizo, M.; Honda, H.; Inagaki, M. Raman spectra of ground natural graphite. Carbon 1978, 16, 281–283. [Google Scholar] [CrossRef]
Figure 1. Geographical location (a), stratigraphic column (b), and sampling (c) of the study area.
Figure 1. Geographical location (a), stratigraphic column (b), and sampling (c) of the study area.
Molecules 27 03810 g001aMolecules 27 03810 g001b
Figure 2. Microscopic coal petrography. (a) ZJ4 sample; (b) ZJ3 sample; (c) ZJ2 sample; (d) ZJ1 sample.
Figure 2. Microscopic coal petrography. (a) ZJ4 sample; (b) ZJ3 sample; (c) ZJ2 sample; (d) ZJ1 sample.
Molecules 27 03810 g002
Figure 3. SEM of coal samples. (a) burrs shapes and radial crack; (b) hot altered hole; (c) burr-like hot pore; (d) calcite fills hydrothermal pore.
Figure 3. SEM of coal samples. (a) burrs shapes and radial crack; (b) hot altered hole; (c) burr-like hot pore; (d) calcite fills hydrothermal pore.
Molecules 27 03810 g003
Figure 4. Changes of pore morphology and mineral composition in coal at different distances from the intrusive rocks. (a) micro-nanometer organic pore; (b) round and smooth pores; (c) high temperature condensation pore; (d) hydrothermal mineral; (e) banded clay minerals; (f) ankerite and pyrite.
Figure 4. Changes of pore morphology and mineral composition in coal at different distances from the intrusive rocks. (a) micro-nanometer organic pore; (b) round and smooth pores; (c) high temperature condensation pore; (d) hydrothermal mineral; (e) banded clay minerals; (f) ankerite and pyrite.
Molecules 27 03810 g004
Figure 5. Relationship between Rmax (%) and Rmin (%).
Figure 5. Relationship between Rmax (%) and Rmin (%).
Molecules 27 03810 g005
Figure 6. Raman spectra of TACG samples and Raman spectrum fitting of the ZJ2 sample. (a) Raman spectra of four graphitized series samples; (b) Raman spectrum fitting results of Z3 sample and the corresponding FWHM parameter settlement principle.
Figure 6. Raman spectra of TACG samples and Raman spectrum fitting of the ZJ2 sample. (a) Raman spectra of four graphitized series samples; (b) Raman spectrum fitting results of Z3 sample and the corresponding FWHM parameter settlement principle.
Molecules 27 03810 g006
Figure 7. Correlation between La and FWG (a) and between La and FWG (b).
Figure 7. Correlation between La and FWG (a) and between La and FWG (b).
Molecules 27 03810 g007
Table 1. Basic data of the coal-based graphite series samples.
Table 1. Basic data of the coal-based graphite series samples.
SampleD (m)Rmin (%)Ro (%)Rmax (%)Proximate AnalysisOrganicInorganic
Ad (%)Vdaf (%)Mad (%)Vitrinite
(%)
Inertinite
(%)
Liptinite
(%)
Clay
(%)
Sulphide
(%)
Carbonate
(%)
ZJ10.13.873.914.6317.468.860.6472.3420.264.111.360.501.43
ZJ20.23.183.554.1719.698.910.6747.6235.8811.172.500.702.13
ZJ30.42.983.123.4117.058.740.5456.3531.027.943.300.460.93
ZJ40.72.562.783.0219.668.060.6262.7023.415.833.370.913.79
D: distance from the sill boundary; d: dry basis; daf: dry-ash-free basis; ad: air-dry basis.
Table 2. Raman spectroscopic parameters of the coal-based graphite series samples.
Table 2. Raman spectroscopic parameters of the coal-based graphite series samples.
SampleBandPosition (D- and G-Peak)ID/IGFWHM (D- and G-Peak)La (Å)
ZJ1D peak13090.27327.272161.2
G peak158020.323
ZJ2D peak13170.37535.259117.3
G peak158320.653
ZJ3D peak13220.49435.80589.1
G peak158426.459
ZJ4D peak13290.61339.96371.8
G peak159128.992
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Luo, H.; Liang, W.; Wei, C.; Wu, D.; Gao, X.; Hu, G. Mineral Composition and Graphitization Structure Characteristics of Contact Thermally Altered Coal. Molecules 2022, 27, 3810. https://doi.org/10.3390/molecules27123810

AMA Style

Luo H, Liang W, Wei C, Wu D, Gao X, Hu G. Mineral Composition and Graphitization Structure Characteristics of Contact Thermally Altered Coal. Molecules. 2022; 27(12):3810. https://doi.org/10.3390/molecules27123810

Chicago/Turabian Style

Luo, Huogen, Wenxu Liang, Chao Wei, Dun Wu, Xia Gao, and Guangqing Hu. 2022. "Mineral Composition and Graphitization Structure Characteristics of Contact Thermally Altered Coal" Molecules 27, no. 12: 3810. https://doi.org/10.3390/molecules27123810

Article Metrics

Back to TopTop