Next Article in Journal
Facile Construction of Hybrid Hydrogels with High Strength and Biocompatibility for Cranial Bone Regeneration
Next Article in Special Issue
Fabrication and Applications of Ceramic-Based Nanofiber Materials Service in High-Temperature Harsh Conditions—A Review
Previous Article in Journal
Influence of Copper-Strontium Co-Doping on Bioactivity, Cytotoxicity and Antibacterial Activity of Mesoporous Bioactive Glass
Previous Article in Special Issue
Hydrophobic Cellulose Acetate Aerogels for Thermal Insulation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Preparation and Properties of Highly Transparent SiO2 Aerogels for Thermal Insulation

1
Institute of Advanced Structure Technology, Beijing Institute of Technology, Beijing 100081, China
2
Beijing Key Laboratory of Lightweight Multi-functional Composite Materials and Structures, Beijing Institute of Technology, Beijing 100081, China
3
Beijing Electro-Mechanical Engineering Institute, Beijing 100074, China
4
Beijing Institute of Spacecraft System Engineering, Beijing 100094, China
*
Author to whom correspondence should be addressed.
Gels 2022, 8(11), 744; https://doi.org/10.3390/gels8110744
Submission received: 3 November 2022 / Revised: 13 November 2022 / Accepted: 15 November 2022 / Published: 16 November 2022
(This article belongs to the Special Issue Gels as High-Performance Thermal Insulation Materials)

Abstract

:
SiO2 aerogels have attracted extensive attention due to their unique structural characteristics, which exhibit many special properties, especially good optical transparency. As far as we know, the sol-gel stage during the synthesis of aerogel plays an important role in the construction of the gel skeleton. In this study, we adjusted the amount of silicon source and catalyst to explore the best scheme for preparing highly transparent SiO2 aerogels, and further clarify the effects of both on the properties of SiO2 aerogels. Results indicated that the pore size distribution was between 10 and 20 nm, the thermal conductivity was between 0.0135 and 0.021 W/(m·K), and the transmittance reached 97.78% at 800 nm of the aerogels, better than most studies. Therefore, it has the potential to be used in aerogel glass for thermal insulation.

1. Introduction

Aerogel [1] is a typical thermal insulation material with a three-dimensional (3D) porous network structure connected by nanoparticles. It has been widely used in numerous fields due to its many unique characteristics and properties, such as low density, high porosity, extremely low thermal conductivity and excellent acoustic properties. SiO2 aerogel [2] with excellent optical transparency has emerged as the most representative aerogel due to its inexpensive cost and straightforward preparation process [3,4,5,6]. Transparent SiO2 aerogel [7,8] has been utilized extensively in Cherenkov detectors [9,10], thermal insulation [11,12,13,14,15], energy-saving [13,16,17,18,19], photoelectric materials [20,21,22], wearables fields [23], thermal collectors [24,25,26,27,28], adsorbents and sensors. Thus, transparent SiO2 aerogel has great research value and the prospects are very broad.
The thermal insulation performance of aerogels has been demonstrated to be due to the low thermal conductivity provided by the high porosity structure [29] and the pore size is preferably smaller than the air free path (70 nm). In addition, high transparency performance requires that the pores of aerogel be much smaller than the wavelength of visible light, so as to minimize the scattering of block. As a result, the porous size of aerogels with thermal insulation as well as highly transparent must be small and uniformly distributed to avoid large deviation of light at the interface of pores. Moreover, SiO2 aerogels are generally prepared by the sol-gel method. Due to the internal disordered porous structure, they are easily cracked and broken during the preparation process, and it is a big challenge to obtain the overall block structure without defects [30]. In most research, the supercritical drying method without gas-liquid interface is used to avoid the generation of capillary forces and reduce the shrinkage of gel.
Researchers have been trying to improve the optical transparency of SiO2 aerogels, but it is exceedingly difficult to combine thermal insulation with high transparency [31,32,33,34]. At present, there are many mainstream or mature strategies to improve the transmittance of SiO2 aerogels. Firstly, in the sol-gel stage, Shimizu et al. [35] found, based on surfactants, that different concentrations of the base catalyst affected the size and uniformity of aerogels skeleton, and thus affected transparency. Zhao et al. [24] proposed a rapid-hydrolysis-condensation procedure and restricted-cluster, and the molar ratio of catalyst was identified as the most critical parameter in the experimental process in order to obtain highly transparent aerogels. Moreover, during the drying process after sol-gel, by controlling shrinkage in the aging process of the gels, Lei et al. [36] prepared polysesiciloxane aerogels with smaller particles and pores. The aerogels with the density of 0.25 g/cm3 had a transmittance of 70% at 550 nm. Similarly, Tabata et al. [9] prepared SiO2 aerogels with higher transparency than conventional methods using a method called pinhole drying [37]. Despite the fact that the transmittance was improved and there were no cracks in the appearance of aerogels, the shrinkage rate of aerogels after drying was very high, which was a common problem in atmospheric drying [1,21]. Finally, after the preparation stage, high-temperature annealing is one of the effective methods to change the microstructure of aerogels. Strobach et al. [25,26] used the viscosity change of aerogels at high temperature to continue to improve transparency. The results showed that aerogels were relatively stable at a low temperature, but particles tend to be extremely aggregated and densified at high temperature. Hence, the size of the scattering source also had a great dependence on temperature, resulting in the increase of transparency. Although temperature treatment can significantly improve transparency, high-temperature treatment is time-consuming and laborious, and will cause shrinkage of aerogels, resulting in an increase in thermal conductivity. In general, the monolithic SiO2 aerogel system became a promising material for windows with highly energy-efficient [12,14,38].
In this paper, we aim to prepare highly transparent SiO2 aerogels with a concise and efficient method. Thus, the alkaline one-step sol-gel method was adopted, and tetramethoxysilane (TMOS), a silicon source with a small molecular volume was selected, and by adjusting the amount of silicon source and alkali catalyst to simply regulated the gel structure. Lastly, the highly transparent SiO2 aerogels were obtained by the appropriate drying method. Here, no additional surfactants and post-treatment were required, the SiO2 aerogels with great advantages in optical transparency were directly obtained through simple processes. Compared to glass, SiO2 aerogels do not generate glare spots, and hold great promise as a means of thermal insulation in the interspace of double-glazing systems as well as in solar collectors.

2. Results and Discussion

2.1. FTIR Spectrum Analysis

Figure 1 showed the FTIR spectrum of SiO2 aerogels, in which 3422 cm−1 was the antisymmetric stretching vibration peak of -OH and 1627 cm−1 was the bending vibration peak of H-O-H; 1094 cm−1 was the antisymmetric stretching vibration peak of the Si-O-Si group, which belonged to the characteristic peak of SiO2, indicating that the main component of sample was SiO2; 957 cm−1 was the stretching vibration peak of Si-OH, and this group was the main reason for the hydrophilicity of SiO2 aerogel; 802 cm−1 was the symmetric stretching vibration peak of Si-O, which also belonged to the characteristic peak of SiO2.

2.2. Microstructure Analysis

The micromorphology of SiO2 aerogels was a typical nano-porous 3D network structure. As shown in Figure 2, when the concentration of NH4OH solution was 0.75 mol/L and the mass fraction of TMOS was 15 wt.%; 25 wt.%; 35 wt.% and 45 wt.%, the micromorphologies with continuous porousity of the prepared SiO2 aerogels were very similar. Small and uniform particles were closely connected with each other through the "neck", and the structure was relatively dense. Due to the different mass fractions of TMOS, the aerogels occurred different shrinkage after drying, as shown in Table 1, resulting in a secondary change in the microstructure. With the decrease in the mass fraction of silicon source, the shrinkage gradually increased, and the structures tended to be dense, which made the structure of SiO2 aerogels with high and low mass fraction very similar, and still maintained a pearl-like 3D network structure. The increase in TMOS content only deepened the densification of the structure slightly. Therefore, the SiO2 aerogels prepared under the condition of different TMOS mass fractions presented a small difference in the micromorphology.
However, When the mass fraction of TMOS was 45 wt.% and the concentration of NH4OH solution was 0.15 mol/L; 0.30 mol/L; 0.45 mol/L; 0.60 mol/L and 0.75 mol/L, the size of SiO2 particles and pores decreased with the increase in the concentration of NH4OH solution, and the structure tended to be denser, as shown in Figure 3. It was attributed to the high catalyst concentration improving the speed of gelation, so that the silicon source can rapidly hydrolyze and condense into primary particles. Then, due to the depletion of the silicon source, the formation of secondary particles lacked raw materials at the later stage, so the clustering process stopped abruptly, resulting in smaller SiO2 particles, smaller pores, and more uniform distribution [24].
Moreover, as shown in Figure 4, the effect of silicon source content and catalyst concentration on the microstructure was also illustrated. Figure 4a showed the N2 adsorption-desorption isotherm curves of SiO2 aerogels which belonged to the type IV, a typical characteristic of mesoporous materials [21]. With the increase in TMOS mass fraction, the specific surface area gradually decreased. On the contrary, with the increase in NH4OH solution concentration, the specific surface area increased accordingly. This was mainly because more silicon sources, the hydrolysis and condensation reaction will be more sufficient, and more SiO2 particles can be generated to secondary particles, as well as the catalyst enabling the reduction of SiO2 particle size by rapid gel process. As shown in Figure 4b, it can be seen that the pore size distribution of each sample was mainly concentrated between 10 and 20 nm, which was divided obviously into two concentrated points due to the different concentration of NH4OH solution. When the concentration of NH4OH solution was low, it was between 15 and 20 nm with wide distribution, and when the concentration of NH4OH solution was high, it is between 10 and 15 nm with narrow distribution. However, the pore size of the NH4OH solution with the same concentration and different TMOS content was roughly the same. Therefore, the effect of NH4OH solution concentration on the pore size distribution was more significant.

2.3. Thermal Properties

As shown in Figure 5a, there are three ways of heat conduction in aerogels: solid-phase heat transfer, gas convection heat transfer, and radiation heat transfer. In general, radiation heat transfer is ignored at room temperature [1]. Figure 5b showed the thermal conductivity of SiO2 aerogels. It can be seen that with the increase in TMOS mass fraction, the thermal conductivity increased, because higher TMOS mass fraction led to higher bulk density, resulting in an increase in the solid-phase heat conduction of the network skeleton. However, the thermal conductivity of 15 wt.% aerogels was slightly higher than that of 25 wt.%. Maybe because too little TMOS content led to larger pores, resulting in higher gas convection heat transfer. At the same time, when the mass fraction of TMOS was same, the thermal conductivity decreased with the increase in the concentration of NH4OH solution. This was owing to a high catalyst concentration, which led to smaller SiO2 particles and pores, which limited the solid-phase heat transfer and gas convection heat transfer, resulting in a lower final thermal conductivity.
Figure 6 showed the infrared thermal imaging of the SiO2 aerogel. It can be seen that the surface temperature of the SiO2 aerogel tended to be stable after 300 s, and the temperature difference ΔT = 44 °C at 600 s, which was about 40% of panel temperature, indicating that the highly transparent SiO2 aerogel had excellent thermal insulation performance.
Table 2 listed the thermal conductivities of SiO2 aerogels, xerogel and cryogel. Through comparison, we found that thanks to the supercritical drying method, SiO2 aerogel had the lowest thermal conductivity and had a great advantage in thermal insulation.

2.4. Optical Transmittance

According to the Rayleigh-Gans theory, the extinction coefficient of aerogels is proportional to the bulk density of aerogels and the diameter of the scattering source [7], as follows:
σ s = 4 π 4 ρ a p ρ S i O 2 d 3 λ 4 ( n 2 1 n 2 2 )
where σ s is scattering coefficient, ρ a p is apparent density or bulk density of SiO2 aerogels, ρ S i O 2 is true density of amorphous silicon (2.2 g/cm3), d is diameter of particle scattering center, λ is wavelength, n is relative refractive index ( n 1 is refractive index of the SiO2 particles, n 2 is refractive index of the external medium (air)). The formulation applies to isolated SiO2 spheres, which approximate a highly porous bulk.
In detail, one of the scattering sources is the macroscopic defects of appearance, which may be caused during the sol-gel process or demolding process [16], so the whole preparation process should try to ensure no pollution and destruction. Another scattering source is the scattering of nano-porous structures, which is the result of the interaction between SiO2 particles and pores [16]. In fact, we can control the density of SiO2 aerogels and the diameter of the scattering source, but because the relationship between the diameter of the scattering source and the extinction coefficient is a power of 3, it becomes a more critical factor.
As shown in Figure 7, SiO2 aerogels themselves have a very low absorption of light. When SiO2 aerogels are irradiated by a beam of light, it may interact with the scattering source in the aerogels and then weaken the intensity of transmittance. According to the Rayleigh-Gans theory, the smaller the size of the SiO2 aerogels structural unit, the smaller the extinction coefficient and the higher the transmittance [41]. Therefore, the optical transparency of SiO2 aerogels was related to the gel structure construction [41,42]. The optimization of composition and microstructure control are effective strategies to improve the high performance and multi-performance of SiO2 aerogels [1].
Figure 8 showed that the transmittance curves of SiO2 aerogels. Figure 8a–d were the transmittance curves under the same TMOS mass fraction and different NH4OH solution concentrations, respectively. According to Figure 8e,f, the results showed that the transmittance of SiO2 aerogels prepared by 45 wt.% TMOS and 0.75 mol/L NH4OH solution were the highest, which reached 97.78% at 800 nm. The reason for that was because the high content of silicon source led to sufficient SiO2 particles generated, while the high concentration of catalyst promoted the hydrolysis and condensation reaction of SiO2, and the cluster was restricted. Under these conditions, the generated SiO2 particles and pores were small and uniform, the scattering source was small, which reduced the deviation of light as well as the scattering of light in the aerogels, so the transparency of aerogels was the highest. The results were consistent with the previous analysis.

3. Conclusions

We used different mass fractions of TMOS and different concentrations of NH4OH solution to simply control the structure of SiO2 aerogels, thereby improving the transmittance. The micromorphology including densification, particle size and pore size distribution of SiO2 aerogels were closely related to the silicon source content and catalyst concentration. After adjusting the experimental parameters, the particles and pore size distribution of SiO2 aerogels were small, and the thermal conductivity was low. More notably, the highest transmittance of SiO2 aerogels can reach 97.78% at 800 nm, which was higher than that of ordinary SiO2 aerogels and undoubtedly broaden the application prospect of SiO2 aerogels in highly transparent materials, such as aerogel glass. However, the mechanical properties and hydrophilicity of highly transparent SiO2 aerogels should be further modified for improvement.

4. Materials and Methods

4.1. Materials

TMOS (AR) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (Shanghai, China). Methanol (AR) was purchased from Beijing Tongguang Fine Chemical Company (Beijing, China). The water (deionized water) was purchased from Shanghai Yien Chemical Technology Co., Ltd. (Shanghai, China). NH4OH (GR) was purchased from Shanghai Maclin Biochemical Technology Co., Ltd. (Shanghai, China). Ethanol (AR) was purchased from Beijing Tongguang Fine Chemical Company (Beijing, China). All chemical regents were used without further purification.

4.2. Preparation of SiO2 Aerogels

The schematic of the preparation process was shown in Figure 9 and the reaction process was shown in Figure 10. The preparation formulations of SiO2 aerogels were listed in Table 3. In the experiments, the mass ratios of TMOS were 15, 25, 35 and 45 wt.%, and the concentrations of NH4OH solution were 0.15, 0.30, 0.45, 0.60 and 0.75 mol/L. Firstly, a certain amount of TMOS and methanol were mixed at room temperature and stirred for 30 min. Then, NH4OH solutions were added and continued to stir until uniform and moved to the mold, which needed to be sealed and placed in a 30 °C oven for 24 h. After the demolding process, the gel was soaked in ethanol for 3 days for solvent replacement and cleaning. Finally, supercritical CO2 drying [43] was performed to obtain highly transparent SiO2 aerogels. The specific parameters of supercritical CO2 drying were set as follows: the temperature of the drying kettle was 32 °C, the temperature of the separating kettle was 37 °C, the pressure of the storage tank was 5.5 MPa, the drying pressure was 7.5 MPa, the separation pressure was 5.5 MPa, and the supercritical state was maintained for about 1 h. Parameters can be adjusted according to different aerogel formulations. Figure 11 showed the pictures of the prepared SiO2 aerogels with difference transparency.

4.3. Characterizations

The microstructure of SiO2 aerogels was observed using a Hitachi S4800 scanning electron microscope. Nitrogen adsorption-desorption tests for observation of pore structure were performed using a Micrometeritics APSP 2460 automatic specific surface area and porosity analyzer. The DRPL-III high-precision thermal conductivity tester was used to test the thermal conductivity of the SiO2 aerogels; the temperature of the hot surface was 40 °C, the temperature of the cold surface was 20 °C, and the pressure was 5 N. A TU-1901 double-beam UV-Vis spectrophotometer was used to perform spectral scanning on the SiO2 aerogels to obtain the transmittance (T%), and the test wavelength range was 200–900 nm. The SiO2 aerogels were formed into a size of 80×80 mm and the thickness was 2–3 mm.

Author Contributions

Conceptualization, L.X., B.M. and B.X.; data curation, B.S. and B.X.; formal analysis, B.S. and L.Q.; funding acquisition, B.X.; investigation, B.S. and Z.Z.; methodology, B.S., B.M. and B.X.; project administration, B.X.; resources, B.X.; supervision, B.X.; visualization, B.S. and B.X.; writing—original draft, B.S.; writing—review & editing, B.S., L.X. and B.X. All authors have read and agreed to the published version of the manuscript.

Funding

This work is supported by the National Key Research and Development of China (No. 2021YFB3400200) and the National Natural Science Foundation of China (No. 12090031).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are available from the authors. Samples of the compounds are available from the authors.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Li, C.; Chen, Z.; Dong, W.; Lin, L.; Zhu, X.; Liu, Q.; Zhang, Y.; Zhai, N.; Zhou, Z.; Wang, Y.; et al. A review of silicon-based aerogel thermal insulation materials: Performance optimization through composition and microstructure. J. Non-Cryst. Solids 2021, 553, 120517. [Google Scholar] [CrossRef]
  2. Karamikamkar, S.; Naguib, H.E.; Park, C.B. Advances in precursor system for silica-based aerogel production toward improved mechanical properties, customized morphology, and multifunctionality: A review. Adv. Coll. Interface Sci. 2020, 276, 102101. [Google Scholar] [CrossRef] [PubMed]
  3. Chen, X.; Zhu, S.; Zhao, B.; Wenbin, Y. Preparation of SiO2 aerogel decived from tetraethyl orthosillicate catalyzed by HCl-NH3. Mod. Chem. Ind. 2003, 23, 147–150. [Google Scholar]
  4. Wang, N.; Ren, H. Investigation process of silica aerogels synthesized by different type of silica recourses. Mater. Rev. 2014, 28, 42–45+58. [Google Scholar]
  5. Cao, D.; Song, D.; Tian, G.; Ding, W. Research Progress on Preparation and Application of Flexible Transparent Silica Aerogels. In Proceedings of the National Thermal Insulation Industry Innovation and Development Seminar & National Thermal Insulation Material Science and Technology Information Association, Guizhou, China, 18–20 October 2019. [Google Scholar]
  6. Liu, J.; Guo, W.; Bai, X.; Chen, D. Research progress on modified silica aerogels. Guangzhou Chem. Ind. 2019, 47, 16–18+27. [Google Scholar] [CrossRef]
  7. Pajonk, G.M. Transparent silica aerogels. J. Non-Cryst. Solids 1998, 225, 307–314. [Google Scholar] [CrossRef]
  8. Chen, W.; Cao, Y.; Ding, W.; Deng, L. Preparation and properties of transparent silica aerogels. In Proceedings of the National Thermal Insulation Industry Innovation and Development Seminar & National Thermal Insulation Material Science and Technology Information Association, Guizhou, China, 18–20 October 2019. [Google Scholar]
  9. Tabata, M.; Adachi, I.; Ishii, Y.; Kawai, H.; Sumiyoshi, T.; Yokogawa, H. Development of transparent silica aerogel over a wide range of densities. Nucl. Instrum. Methods Phys. Res. Sect. A 2010, 623, 339–341. [Google Scholar] [CrossRef] [Green Version]
  10. Tsou, P. Silica aerogel captures cosmic dust intact. J. Non-Cryst. Solids 1995, 186, 415–427. [Google Scholar] [CrossRef]
  11. Hu, F.; An, L.; Li, C.; Liu, J.; Ma, G.; Hu, Y.; Huang, Y.; Liu, Y.; Thundat, T.; Ren, S. Transparent and flexible thermal insulation window material. Cell Rep. Phys. Sci. 2020, 1, 100140. [Google Scholar] [CrossRef]
  12. Jensen, K.I.; Schultz, J.M.; Kristiansen, F.H. Development of windows based on highly insulating aerogel glazings. J. Non-Cryst. Solids 2004, 350, 351–357. [Google Scholar] [CrossRef]
  13. Liu, Q.; Frazier, A.W.; Zhao, X.; De La Cruz, J.A.; Hess, A.J.; Yang, R.; Smalyukh, I.I. Flexible transparent aerogels as window retrofitting films and optical elements with tunable birefringence. Nano Energy 2018, 48, 266–274. [Google Scholar] [CrossRef]
  14. Marszewski, M.; King, S.C.; Yan, Y.; Galy, T.; Li, M.; Dashti, A.; Butts, D.M.; Kang, J.S.; McNeil, P.E.; Lan, E.; et al. Thick transparent nanoparticle-based mesoporous silica monolithic slabs for thermally insulating window materials. ACS Appl. Nano Mater. 2019, 2, 4547–4555. [Google Scholar] [CrossRef]
  15. Zheng, D.; Chen, Y.; Liu, Y.; Li, Y.; Zheng, S.; Lu, B. Experimental comparisons on optical and thermal performance between aerogel glazed skylight and double glazed skylight under real climate condition. Energy Build. 2020, 222, 110028. [Google Scholar] [CrossRef]
  16. Wang, J.; Petit, D.; Ren, S. Transparent thermal insulation silica aerogels. Nanoscale Adv. 2020, 2, 5504–5515. [Google Scholar] [CrossRef]
  17. Wei, T.; Lu, S.; Chang, Y. Transparent, hydrophobic composite aerogels with high mechanical strength and low high-temperature thermal conductivities. J. Phys. Chem. B 2008, 112, 11881–11886. [Google Scholar] [CrossRef]
  18. Baetens, R.; Jelle, B.P.; Gustavsen, A. Aerogel insulation for building applications: A state-of-the-art review. Energy Build. 2011, 43, 761–769. [Google Scholar] [CrossRef] [Green Version]
  19. Sun, Y.; Wilson, R.; Wu, Y. A Review of transparent insulation material (TIM) for building energy saving and daylight comfort. Appl. Energy 2018, 226, 713–729. [Google Scholar] [CrossRef]
  20. Zu, G.; Shimizu, T.; Kanamori, K.; Zhu, Y.; Maeno, A.; Kaji, H.; Shen, J.; Nakanishi, K. Transparent, superflexible doubly cross-linked polyvinylpolymethylsiloxane aerogel superinsulators via ambient pressure drying. ACS Nano 2018, 12, 521–532. [Google Scholar] [CrossRef]
  21. He, P.; Gao, X.; Li, X.; Jiang, Z.; Yang, Z.; Wang, C.; Gu, Z. Highly transparent silica aerogel thick films with hierarchical porosity from water glass via ambient pressure drying. Mater. Chem. Phys. 2014, 147, 65–74. [Google Scholar] [CrossRef]
  22. Zu, G.; Kanamori, K.; Shimizu, T.; Zhu, Y.; Maeno, A.; Kaji, H.; Nakanishi, K.; Shen, J. Versatile double-cross-linking approach to transparent, machinable, supercompressible, highly bendable aerogel thermal superinsulators. Chem. Mater. 2018, 30, 2759–2770. [Google Scholar] [CrossRef] [Green Version]
  23. Du, Y.; Zhang, X.; Wang, J.; Liu, Z.; Zhang, K.; Ji, X.; You, Y.; Zhang, X. Reaction-spun transparent silica aerogel fibers. ACS Nano 2020, 14, 11919–11928. [Google Scholar] [CrossRef] [PubMed]
  24. Zhao, L.; Bhatia, B.; Yang, S.; Strobach, E.; Weinstein, L.A.; Cooper, T.A.; Chen, G.; Wang, E.N. Harnessing heat beyond 200 °C from unconcentrated sunlight with nonevacuated transparent aerogels. ACS Nano 2019, 13, 7508–7516. [Google Scholar] [CrossRef] [PubMed]
  25. Strobach, E.; Bhatia, B.; Yang, S.; Zhao, L.; Wang, E.N. High temperature stability of transparent silica aerogels for solar thermal applications. APL Mater. 2019, 7, 081104. [Google Scholar] [CrossRef] [Green Version]
  26. Strobach, E.; Bhatia, B.; Yang, S.; Zhao, L.; Wang, E.N. High temperature annealing for structural optimization of silica aerogels in solar thermal applications. J. Non-Cryst. Solids 2017, 462, 72–77. [Google Scholar] [CrossRef] [Green Version]
  27. Zhao, L.; Bhatia, B.; Cooper, T.; Strobach, E.; Yang, S.; Weinstein, L.A.; Chen, G.; Wang, E.N. Intermediate temperature solar thermal collector enabled by non-evacuated transparent aerogel and non-tracking compound parabolic concentrator. In Proceedings of the 16th International Heat Transfer Conference, Beijing, China, 10–15 August 2018. [Google Scholar] [CrossRef]
  28. Ammar, M.; Mokni, A.; Mhiri, H.; Bournot, P. Performance optimization of flat plate solar collector through the integration of different slats arrangements made of transparent insulation material. Sustain. Energy Technol. Assess. 2021, 46, 101237. [Google Scholar] [CrossRef]
  29. Guzel Kaya, G.; Deveci, H. Effect of aging solvents on physicochemical and thermal properties of silica xerogels derived from steel slag. Chem. Sel. 2020, 5, 1586–1591. [Google Scholar] [CrossRef]
  30. Wang, L.; Feng, J.; Luo, Y.; Zhou, Z.; Jiang, Y.; Luo, X.; Xu, L.; Li, L.; Feng, J. Three-dimensional-printed silica aerogels for thermal insulation by directly writing temperature-induced solidifiable Inks. ACS Appl. Mater. Interfaces 2021, 13, 40964–40975. [Google Scholar] [CrossRef]
  31. Li, X.; Yang, Z.; Li, K.; Zhao, S.; Fei, Z.; Zhang, Z. Preparation and characterization of transparent and compressible methylsilsesquioxane aerogels using MTES as precursor. Chem. Ind. Eng. Prog. 2020, 39, 1115–1121. [Google Scholar] [CrossRef]
  32. Liu, W. Studies of Preparation and Performance of Transparent Silica Aerogel. Master’s Thesis, Southwest University of Science and Technology, Mianyang, China, 2016. [Google Scholar]
  33. Du, A.; Wang, H.; Zhou, B.; Zhang, C.; Wu, X.; Ge, Y.; Niu, T.; Ji, X.; Zhang, T.; Zhang, Z.; et al. Multifunctional silica nanotube aerogels inspired by polar bear hair for light management and thermal insulation. Chem. Mater. 2018, 30, 6849–6857. [Google Scholar] [CrossRef]
  34. Parale, V.G.; Lee, K.Y.; Park, H.H. Flexible and transparent silica aerogels: An overview. J. Korean Ceram. Soc. 2017, 54, 184–199. [Google Scholar] [CrossRef] [Green Version]
  35. Shimizu, T.; Kanamori, K.; Maeno, A.; Kaji, H.; Doherty, C.M.; Falcaro, P.; Nakanishi, K. Transparent, highly insulating polyethyl- and polyvinylsilsesquioxane aerogels: Mechanical improvements by vulcanization for ambient pressure drying. Chem. Mater. 2016, 28, 6860–6868. [Google Scholar] [CrossRef]
  36. Lei, C.; Li, J.; Sun, C.; Yang, H.; Xia, T.; Hu, Z.; Zhang, Y. Transparent, elastic and crack-free polymethylsilsesquioxane aerogels prepared by controllable shrinkage of the hydrogels in the aging process. Microporous Mesoporous Mater. 2018, 267, 107–114. [Google Scholar] [CrossRef]
  37. Li, T.; Zhou, B.; Du, A.; Xiang, Y.; Wu, S.; Liu, M.; Ding, W.; Shen, J.; Zhang, Z. Microstructure control of the silica aerogels via pinhole drying. J. Sol-Gel Sci. Technol. 2017, 84, 96–103. [Google Scholar] [CrossRef]
  38. Bhuiya, M.M.H.; Anderson, A.M.; Carroll, M.K.; Bruno, B.A.; Ventrella, J.L.; Silberman, B.; Keramati, B. Preparation of monolithic silica aerogel for fenestration applications: Scaling up, reducing cycle time, and improving performance. Ind. Eng. Chem. Res. 2016, 55, 6971–6981. [Google Scholar] [CrossRef]
  39. Su, L.; Miao, L.; Xu, G.; Tanemura, S. Super Thermal insulating SiO2 cryogels prepared by vacuum freeze drying. Adv. Mater. Res. 2010, 105, 851–854. [Google Scholar] [CrossRef]
  40. Chen, M. Study on Preparation of SiO2 Series Xerogels. Master’s Thesis, Hebei Polytechnic University, Tangshan, China, 2009. [Google Scholar]
  41. Emmerling, A.; Petricevic, R.; Beck, A.; Wang, P.; Scheller, H.; Fricke, J. Relationship between optical transparency and nanostructural features of silica aerogels. J. Non-Cryst. Solids 1995, 185, 240–248. [Google Scholar] [CrossRef]
  42. Ji, X.; Du, Y.; Zhang, X. Elaborate size-tuning of silica aerogel building blocks enables laser-driven lighting. Adv. Mater. 2022, 34, 2107168. [Google Scholar] [CrossRef]
  43. Li, J.; Zhao, Y.; Ren, F.; Wang, J. Preparation of silica aerogel by different supercritical drying processes. Archit. Technol. 2019, 50, 981–984. [Google Scholar] [CrossRef]
Figure 1. FTIR spectrum of SiO2 aerogels.
Figure 1. FTIR spectrum of SiO2 aerogels.
Gels 08 00744 g001
Figure 2. SEM of SiO2 aerogels: the concentration of NH4OH solution was 0.75 mol/L and the mass fractions of TMOS were (a) 15 wt.%; (b) 25 wt.%; (c) 35 wt.%; (d) 45 wt.%.
Figure 2. SEM of SiO2 aerogels: the concentration of NH4OH solution was 0.75 mol/L and the mass fractions of TMOS were (a) 15 wt.%; (b) 25 wt.%; (c) 35 wt.%; (d) 45 wt.%.
Gels 08 00744 g002
Figure 3. SEM of SiO2 aerogels: the mass fraction of TMOS was 45 wt.% and the concentration of NH4OH solutions were (a) 0.15 mol/L; (b) 0.30 mol/L; (c) 0.45 mol/L; (d) 0.60 mol/L; (e) 0.75 mol/L.
Figure 3. SEM of SiO2 aerogels: the mass fraction of TMOS was 45 wt.% and the concentration of NH4OH solutions were (a) 0.15 mol/L; (b) 0.30 mol/L; (c) 0.45 mol/L; (d) 0.60 mol/L; (e) 0.75 mol/L.
Gels 08 00744 g003
Figure 4. (a) N2 adsorption-desorption isotherm curves of SiO2 aerogels; (b) pore size distribution curves of SiO2 aerogels.
Figure 4. (a) N2 adsorption-desorption isotherm curves of SiO2 aerogels; (b) pore size distribution curves of SiO2 aerogels.
Gels 08 00744 g004
Figure 5. (a) The heat transfer modes in aerogels; (b) thermal conductivity curves of SiO2 aerogels.
Figure 5. (a) The heat transfer modes in aerogels; (b) thermal conductivity curves of SiO2 aerogels.
Gels 08 00744 g005
Figure 6. The infrared thermal imaging of the SiO2 aerogel.
Figure 6. The infrared thermal imaging of the SiO2 aerogel.
Gels 08 00744 g006
Figure 7. The propagation paths of light in SiO2 aerogels.
Figure 7. The propagation paths of light in SiO2 aerogels.
Gels 08 00744 g007
Figure 8. Transmittance curves of SiO2 aerogels with different TMOS mass fractions: (a) 15 wt.%; (b) 25 wt.%; (c) 35 wt.%; (d) 45 wt.%; (e) the highest transmittance among the TMOS mass fractions of 15–45 wt.% and its (f) local magnification of wavelengths from 750 nm to 850 nm.
Figure 8. Transmittance curves of SiO2 aerogels with different TMOS mass fractions: (a) 15 wt.%; (b) 25 wt.%; (c) 35 wt.%; (d) 45 wt.%; (e) the highest transmittance among the TMOS mass fractions of 15–45 wt.% and its (f) local magnification of wavelengths from 750 nm to 850 nm.
Gels 08 00744 g008
Figure 9. Schematic of preparation process of highly transparent SiO2 aerogels.
Figure 9. Schematic of preparation process of highly transparent SiO2 aerogels.
Gels 08 00744 g009
Figure 10. (a) Hydrolysis reaction of TMOS; (b) condensation reaction of TMOS after hydrolysis; (c) further cross-linking by condensation reaction to form a 3D network.
Figure 10. (a) Hydrolysis reaction of TMOS; (b) condensation reaction of TMOS after hydrolysis; (c) further cross-linking by condensation reaction to form a 3D network.
Gels 08 00744 g010
Figure 11. Pictures of SiO2 aerogels with difference transparency: (a) sample 12 and (b) sample 20.
Figure 11. Pictures of SiO2 aerogels with difference transparency: (a) sample 12 and (b) sample 20.
Gels 08 00744 g011
Table 1. Shrinkage of SiO2 aerogels with different mass fractions of TMOS.
Table 1. Shrinkage of SiO2 aerogels with different mass fractions of TMOS.
TMOS (wt.%)15253545
Line Shrinkage (%)22~2711~158~105~9
Table 2. The thermal conductivities of SiO2 aerogels, xerogel and cryogel [29,30,39,40].
Table 2. The thermal conductivities of SiO2 aerogels, xerogel and cryogel [29,30,39,40].
SamplesSiO2 AerogelSiO2 XerogelSiO2 Cryogel
Thermal conductivity (W/(m·K))0.01–0.030.03–0.090.03–0.05
Table 3. Preparation formulations of highly transparent SiO2 aerogels.
Table 3. Preparation formulations of highly transparent SiO2 aerogels.
SamplesTMOS (wt.%)TMOS (g)Methanol (g)NH4OH (g)Deionized Water (g)
1152.4710.40.0193.6
20.038
30.058
40.077
50.097
6254.6710.40.0193.6
70.038
80.058
90.077
100.097
11357.5310.40.0193.6
120.038
130.058
140.077
150.097
164511.4510.40.0193.6
170.038
180.058
190.077
200.097
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Shi, B.; Xie, L.; Ma, B.; Zhou, Z.; Xu, B.; Qu, L. Preparation and Properties of Highly Transparent SiO2 Aerogels for Thermal Insulation. Gels 2022, 8, 744. https://doi.org/10.3390/gels8110744

AMA Style

Shi B, Xie L, Ma B, Zhou Z, Xu B, Qu L. Preparation and Properties of Highly Transparent SiO2 Aerogels for Thermal Insulation. Gels. 2022; 8(11):744. https://doi.org/10.3390/gels8110744

Chicago/Turabian Style

Shi, Baolu, Long Xie, Bin Ma, Zhiliang Zhou, Baosheng Xu, and Lijie Qu. 2022. "Preparation and Properties of Highly Transparent SiO2 Aerogels for Thermal Insulation" Gels 8, no. 11: 744. https://doi.org/10.3390/gels8110744

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop