Proceeding Paper

Highly Sensitive NH3 Sensors Using CVD and Epitaxial Graphene Functionalised with Vanadium(V) Oxide: A Comparative Study †

1
Institute of Physics, University of Tartu, W. Ostwald Street 1, EE50411 Tartu, Estonia
2
Department of Physics, Chemistry and Biology, Linköping University, 58183 Linköping, Sweden
*
Author to whom correspondence should be addressed.
Presented at the Eurosensors 2018 Conference, Graz, Austria, 9–12 September 2018.
Proceedings 2018, 2(13), 854; https://doi.org/10.3390/proceedings2130854
Published: 20 November 2018
(This article belongs to the Proceedings of EUROSENSORS 2018)

Abstract

:
Exceptionally sensitive and selective graphene-based chemiresistive gas sensors were produced as a result of graphene functionalisation with a sub-nanometer V2O5 layer by using the method of pulsed laser deposition. Two different types of graphene were used—epitaxial graphene on SiC and CVD graphene on Si/SiO2—and both showed remarkable enhancement of sensing properties in terms of response and recovery speed, response magnitude and selectiveness towards NH3 gas. The epitaxial graphene-based sensor was demonstrating the highest relative response towards ammonia amounting to 80% for 0.1 ppm NH3.

1. Introduction

Since its discovery, graphene as a monolayer-thick (semi)conducting material was investigated as a gas sensing system, with great potential for miniaturization, low-power operation and cheap production [1]. However, realization of practical sensing systems functioning in real atmosphere with the high concentration of oxygen and water vapor is still challenging. Enhancement of sensing properties of graphene is possible by promoting gas adsorption through introducing defects, atomic dopants, or by functionalisation with nanoparticles [2]. A pulsed laser deposition of a sub-nanometer thick layer of catalytically active V2O5 gives CVD graphene remarkable sensitivity and selectivity towards ammonia gas [3]. Even greater improvement would be expected in the case of epitaxial graphene, because of its higher sensitivity to chemical doping as a result of its lower intrinsic doping level [4].
In the current work, the chemical vapour deposited graphene on Si/SiO2 (Si/SiO2/CVDG), and the epitaxial graphene grown on SiC (SiC/EG) were functionalised by laser deposited ultra-thin (0.6 nm) V2O5 layer. The effect of PLD process on graphene defect creation was investigated by Raman spectroscopy. The NH3 gas sensing properties are compared for pristine and V2O5 deposited graphenes. Responses of both types of graphene sensors to other polluting gases NO2, CO, SO2 and O3 were researched to test the selectivity.

2. Materials and Methods

Chemical vapour deposited graphene was grown on a commercial 25 µm thick polycrystalline copper foil in a home-built CVD reactor. The grown graphene film was transferred onto Si/SiO2 substrate carrying Au (60 nm) electrodes deposited through a shadow mask by magnetron sputtering. The graphene growth and transfer processes were executed as described earlier [3]. Epitaxial graphene (EG) was grown by sublimation method on Si-terminated 4H–SiC (0001) substrates at 2000 °C in argon gas at 1 bar [5]. Au (200 nm) contact pads were made by evaporation on top of SiC/EG substrate. In the PLD process, a ceramic V2O5 target was ablated with a KrF excimer laser at wavelength 248 nm and laser pulse energy density of 5.0 J/cm2, in the presence of 5 × 10−2 mbar of O2. The total of 120 laser pulses with a repetition rate of 5 Hz was used for V2O5 layer deposition. Sensor substrates were kept at the room temperature during deposition.
Gas sensitivity was measured the room temperature in a 7 cm3 stainless steel sample chamber, equipped with a gas mixing system [6]. The voltage applied to the electrodes was 100 mV. In the experiments with UV light excitation, the 365 nm light intensity on the sample was ~15 mW/cm2.

3. Results and Discussion

According to the analysis of vanadium valence state by X-ray photoelectron spectroscopy (XPS) and a mass thickness measurement by X-ray fluorescence (XRF), the material deposited on graphene is predominately in the highest stable oxidation state of vanadium, V2O5, and has an average thickness of ~0.6 nm [3].
As indicated by the Raman spectrum (Figure 1), the defectiveness of CVD graphene increased drastically as a result of PLD, which is an expected result of high energy atomic bombardment with PLD plasma species. The rise of defectiveness by PLD is evident from the emergence of prominent defect-related D and D’ bands, and a height decrease of G and 2D bands at the same time. By contrary, for EG on SiC substrate the typical Raman peaks indicate that graphene remained intact after identical PLD treatment. This implies a much larger resilience against the defect creation, probably due to much tighter graphene-to-support contact in case of EG on SiC. This interpretation is also supported by the fact that the electrical conductivity of SiC/EG sample did not change after the PLD of V2O5, whereas the conductivity of CVD graphene sample dropped substantially.
Compared to unmodified graphene, large improvement of sensor response to the reducing NH3 gas was achieved for both types of graphene sensors (Figure 2). The SiC/EG showed by an order of magnitude larger response, as compared to CVDG sensor. For instance, the relative response to 100 ppm NH3 was 295% and 31% in case of EG and CVDG sensors, respectively. The conductivity of different types of graphene sensors changes in opposite direction after introducing NH3, due to different types of majority charge carriers—electrons in Si/SiO2/CVDG and holes in SiC/EG.
In addition, considerably faster characteristic response times were measured on both types of sensors after deposition (by 4 to 6 times). Again, the improvement of the response and recovery speed was more drastic for the SiC/EG sensor. Enhancement of gas response can be caused by increased density of energetically favourable adsorption sites or/and increased charge transfer from NH3 adsorbate molecules [4]. Strong adsorption ability of NH3 on V2O5 and possible redox reactions on the surface of V2O5 are well known [7]. Although perfect graphene is relatively inert with respect to chemisorption, owing to low concentration of dangling bonds and lack of charged atoms on the surface [2], the as-made, or pristine graphene almost always shows considerable gas sensitivity to NO2 and NH3, in conjunction with extremely slow sensor recovery at RT [1,2,8]. High adsorption energy binding sites may exist in freshly produced graphene, such as uncontrollably introduced defects or dopant atoms in the graphene lattice. In the course of functionalisation a high number of point defects is formed by bombardment with high-energy atoms of PLD plasma. The induced defects are further modified through the adding of functionalising oxide material [3,9].
The recovery kinetics and the dependence of sensor response magnitudes on NH3 concentration are in accordance with Langmuir type two-site adsorption model [10]:
S x = G x G 0 G 0 = α 1 x b 1 1 + x b 1 + α 2 x b 2 1 + x b 2 ,
where b1 and b2 are affinity constants, α1 and α2 are transduction coefficients.
Fitting the data with the model resulted in two important consequences regarding functionalised graphene sensors:
  • Adsorption sites with comparable affinity constants b1 and b2 on both types of graphene indicate the similar effect of deposited V2O5 nanophase on the surface.
  • Both transduction coefficients α1 and α2 are much smaller in case of CVD graphene sensor, which means less influence of gas adsorption on relative conductivity, and hence, lower relative gas response of the CVD graphene sensor. Taking into account that the gas adsorption mainly modifies the charge carrier concentration rather than mobility [1], the substantially larger response of EG sensor is probably arising from lower initial carrier doping of EG as compared to free electron concentration in CVD graphene.
The selectivity with respect to NH3 of both CVDG and EG sensors increases after the PLD of V2O5, when compared to the response to several other polluting gases. For instance, in case of EG, the response to NH3 increases significantly by functionalisation, and at the same time, the response to NO2 gas is reduced, thus improving the selectivity. The functionalisation with V2O5 slightly increases the response to CO and SO2 gases for both types of sensors, both gases being reducing. As expected from the strongly oxidizing properties, reactions to O3 and NO2 gases are much alike.

4. Conclusions

CVD-grown graphene (Si/SiO2/CVDG) and the epitaxial graphene grown on SiC (SiC/EG) were functionalised by laser deposited ultra-thin V2O5 layer (0.6 nm). Compared to pristine graphene sensors, large and selective enhancement of sensor response to the reducing NH3 gas was achieved for both types of graphenes. The effect of metal oxide modifier was more remarkable for EG which showed, as compared to similarly functionalised CVDG sensor, by an order of magnitude larger response (295% vs. 31% for 100 ppm NH3). The recovery kinetics and dependence on NH3 concentration are in accordance with Langmuir type two-site adsorption model. The results imply the presence of similar adsorption sites on both types of materials, indicating a similar role of deposited V2O5 nanophase on the surface. The substantially larger response of EG sensor is probably the result of the lower initial carrier doping in EG.

Acknowledgments

This project has received funding from the European Union’s Horizon 2020 research and innovation program under the grant agreement No 785219 and was supported by institutional research fund IUT34-27 of the Estonian Ministry of Education and Science. J.E. and R.Y. would like to thank financial support from the Swedish Foundation for Strategic Research (SSF), through the grants GMT14-0077 and RMA15-024.

Conflicts of Interest

The authors declare no conflict of interest. The founding sponsors had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, and in the decision to publish the results.

References

  1. Schedin, F.; Geim, A.K.; Morozov, S.V.; Hill, E.W.; Blake, P.; Katsnelson, M.I.; Novoselov, K.S. Detection of individual gas molecules adsorbed on graphene. Nat. Mater. 2007, 6, 652–655. [Google Scholar] [CrossRef]
  2. Lee, G.; Yang, G.; Cho, A.; Han, J.W.; Kim, J. Defect-engineered graphene chemical sensors with ultrahigh sensitivity. Phys. Chem. Chem. Phys. 2016, 18, 14198–14204. [Google Scholar] [CrossRef]
  3. Kodu, M.; Berholts, A.; Kahro, T.; Kook, M.; Ritslaid, P.; Seemen, H.; Avarmaa, T.; Alles, H.; Jaaniso, R. Graphene functionalised by laser-ablated V2O5 for a highly sensitive NH3 sensor. Beilstein J. Nanotechnol. 2017, 8, 571–578. [Google Scholar] [CrossRef] [PubMed]
  4. Jaaniso, R.; Tan, O.K. Semiconductor Gas Sensors; Woodhead Publishing: Cambridge, UK, 2013; p. 147. [Google Scholar]
  5. Yakimova, R.; Virojanadara, C.; Gogova, D.; Syväjärvi, M.; Siche, D.; Larsson, K.; Johansson, L.I. Analysis of the formation conditions for large area epitaxial graphene on SiC substrates. Mater. Sci. Forum 2010, 645–648, 565–568. [Google Scholar] [CrossRef]
  6. Berholts, A.; Kahro, T.; Floren, A.; Alles, H.; Jaaniso, R. Photo-activated oxygen sensitivity of graphene at room temperature. Appl. Phys. Lett. 2014, 105, 163111. [Google Scholar] [CrossRef]
  7. Sun, D.; Liu, Q.; Liu, Z.; Gui, G.; Huang, Z. Adsorption and oxidation of NH3 over V2O5/AC surface. Appl. Catal. B 2009, 92, 462–467. [Google Scholar] [CrossRef]
  8. Eriksson, J.; Puglisi, D.; Kang, Y.H.; Yakimova, R.; Lloyd Spetz, A. Adjusting the electronic properties and gas reactivity of epitaxial graphene by thin surface metallization. Phys. B Condens. Matter 2014, 439, 105–108. [Google Scholar] [CrossRef]
  9. Kodu, M.; Berholts, A.; Kahro, T.; Avarmaa, T.; Kasikov, A.; Niilisk, A.; Alles, H.; Jaaniso, R. Highly sensitive NO2 sensors by pulsed laser deposition on graphene. Appl. Phys. Lett. 2016, 109, 113108. [Google Scholar] [CrossRef]
  10. Jaaniso, R.; Kahro, T.; Kozlova, J.; Aarik, J.; Aarik, L.; Alles, H.; Floren, A.; Gerst, A.; Kasikov, A.; Niilisk, A.; et al. Temperature induced inversion of oxygen response in CVD graphene on SiO2. Sens. Actuators B Chem. 2014, 190, 1006–1013. [Google Scholar] [CrossRef]
Figure 1. Typical Raman spectra of CVD and epitaxial graphene in the sensor devices, recorded between the electrodes before and after the laser deposition of V2O5: strong defect-related peaks D and D’ after deposition on CVDG did not appear noticeably in case of SiC/EG.
Figure 1. Typical Raman spectra of CVD and epitaxial graphene in the sensor devices, recorded between the electrodes before and after the laser deposition of V2O5: strong defect-related peaks D and D’ after deposition on CVDG did not appear noticeably in case of SiC/EG.
Proceedings 02 00854 g001
Figure 2. Influence of graphene functionalisation with V2O5 on gas sensitivity and selectivity: (a) Electric conduction response of CVD graphene on Si/SiO2 and EG on SiC to different NH3 concentrations at room temperature. Results for pristine graphenes are shown as a reference. Permanent UV light was on during the measurements. Relative humidity was 20%. All time intervals of gas exposure and recovery are 900 s; (b) Sensor response amplitudes to different polluting gases of CVD graphene (CVDG) and epitaxial graphene (EG) sensors with and without laser deposited V2O5 layer.
Figure 2. Influence of graphene functionalisation with V2O5 on gas sensitivity and selectivity: (a) Electric conduction response of CVD graphene on Si/SiO2 and EG on SiC to different NH3 concentrations at room temperature. Results for pristine graphenes are shown as a reference. Permanent UV light was on during the measurements. Relative humidity was 20%. All time intervals of gas exposure and recovery are 900 s; (b) Sensor response amplitudes to different polluting gases of CVD graphene (CVDG) and epitaxial graphene (EG) sensors with and without laser deposited V2O5 layer.
Proceedings 02 00854 g002
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Kodu, M.; Berholts, A.; Kahro, T.; Eriksson, J.; Yakimova, R.; Avarmaa, T.; Renge, I.; Alles, H.; Jaaniso, R. Highly Sensitive NH3 Sensors Using CVD and Epitaxial Graphene Functionalised with Vanadium(V) Oxide: A Comparative Study. Proceedings 2018, 2, 854. https://doi.org/10.3390/proceedings2130854

AMA Style

Kodu M, Berholts A, Kahro T, Eriksson J, Yakimova R, Avarmaa T, Renge I, Alles H, Jaaniso R. Highly Sensitive NH3 Sensors Using CVD and Epitaxial Graphene Functionalised with Vanadium(V) Oxide: A Comparative Study. Proceedings. 2018; 2(13):854. https://doi.org/10.3390/proceedings2130854

Chicago/Turabian Style

Kodu, Margus, Artjom Berholts, Tauno Kahro, Jens Eriksson, Rositsa Yakimova, Tea Avarmaa, Indrek Renge, Harry Alles, and Raivo Jaaniso. 2018. "Highly Sensitive NH3 Sensors Using CVD and Epitaxial Graphene Functionalised with Vanadium(V) Oxide: A Comparative Study" Proceedings 2, no. 13: 854. https://doi.org/10.3390/proceedings2130854

Article Metrics