Article

Enhancement of InSe Field-Effect-Transistor Performance against Degradation of InSe Film in Air Environment

1
Key Laboratory of Microelectronics Device & Integrated Technology, Institute of Microelectronics Chinese Academy of Sciences, Beijing 100029, China
2
School of Information Engineering, Hebei University of Technology, Tianjin 300401, China
3
University of Chinese Academy of Sciences, Beijing 100049, China
*
Authors to whom correspondence should be addressed.
Nanomaterials 2021, 11(12), 3311; https://doi.org/10.3390/nano11123311
Submission received: 12 November 2021 / Revised: 26 November 2021 / Accepted: 30 November 2021 / Published: 6 December 2021
(This article belongs to the Topic Advances and Applications of 2D Materials)

Abstract

:
The degradation of InSe film and its impact on field effect transistors are investigated. After the exposure to atmospheric environment, 2D InSe flakes produce irreversible degradation that cannot be stopped by the passivation layer of h-BN, causing a rapid decrease for InSe FETs performance, which is attributed to the large number of traps formed by the oxidation of 2D InSe and adsorption to impurities. The residual photoresist in lithography can cause unwanted doping to the material and reduce the performance of the device. To avoid contamination, a high-performance InSe FET is achieved by a using hard shadow mask instead of the lithography process. The high-quality channel surface is manifested by the hysteresis of the transfer characteristic curve. The hysteresis of InSe FET is less than 0.1 V at Vd of 0.2, 0.5, and 1 V. And a high on/off ratio of 1.25 × 108 is achieved, as well relative high Ion of 1.98 × 10−4 A and low SS of 70.4 mV/dec at Vd = 1 V are obtained, demonstrating the potential for InSe high-performance logic device.

1. Introduction

Recently, increasing attention has been attracted by two-dimensional (2D) materials, including transition metal dichalcogenides (TMDs), Ⅲ-Ⅵ layered semiconductors (InSe, In2Se3), black phosphorus and graphene, for their potential applications in photo electronic devices, field effect transistors (FETs), integrated circuits and three-dimensional integrated circuit (3D-IC) [1,2,3,4,5]. With the rapid development of the semiconductor process, silicon-based semiconductor materials will not be able to meet the requirements of transistor size reduction in the foreseeable future, especially when the performance of FETs determines the performance of integrated circuits [6]. Conventional high mobility channel materials like InGaAs, Ge also encounter great challenges of strong quantum effect in nanometer scale [7,8], which makes them gradually lose the opportunity in advanced technology node even regardless of the process difficulties. As promising alternative materials for current silicon-based semiconductor devices, the unique layered structure of two-dimensional materials has excellent electrical and optical properties, which makes 2D materials suitable candidates for compact, ultrathin, and high-performance next-generation logic nanodevices [9,10,11]. InSe, which belongs to the family of metal chalcogenide layer semiconductors, is an attractive material in the field of electronics because of its direct and moderate band gap of 1.26 eV of monolayer, ultra-high mobility of 1000 cm2·V−1·s−1 at room temperature, which can be further optimized by strain engineering [12]. Compared with graphene, which is of high mobility but vanished band gap, InSe is more suitable as the channel material for FETs [13]. However, the excellent performance of InSe can be easily hidden by oxidation and impurities absorption when it is exposed to ambient environment and even when the InSe FET is fabricated. In practical applications, this can seriously affect the performance and stability of InSe FETs. To obtain high-performance InSe FET, many passivation layers are chosen to cap on the channel surface, such as indium [14], h-BN [15], HfO2 [16], and In2O3 [17]. However, the hysteresis of InSe FET can hardly be eliminated, which also degrades the performance of logic devices. According to the properties of InSe materials, the decay of materials and FETs in air environment is studied, which is necessary for device process improvement and promoting performance.
In this work, we characterized InSe materials and FETs, finding that the degradation of InSe is unstoppable, but it can be mitigated through the passivation of h-BN on the top of InSe film. A high-performance InSe field effect transistor without hysteresis was fabricated using a modified method, demonstrating the great application prospect of InSe field effect transistors in integrated circuits.

2. Materials and Methods

In the device fabrication, a p-type Si wafer (8-inch) was cleaned with the standard clean method to remove the intrinsic silicon oxide layer on the surface and was used as the substrate, which also served as the back-gate electrode of the InSe FET. The back-gate dielectric of 20 nm HfO2 film was deposited by atomic layer deposition (ALD) with Hf[N(C2H5)CH3]4 (TEMAH) and H2O as Hf and oxygen precursors. The injection sequence of the reaction chamber is TEMAH-2-H2O-N2 in which N2 is purge gas and its purpose is to remove the excess gas and other by-products. Next, the rapid thermal annealing (RTA) process was implemented at 450 ℃ for 15 s to improve the dielectric film quality [18].
The InSe flakes were obtained by mechanical exfoliation using Scotch tape. Firstly, the bulk InSe (purchased from Six Carbon Technology) was thinned using tape. Then, the tape was attached to the target substrate and torn off to complete InSe flakes transfer. After that, we used lithography to define the source and drain contact region and Ti/Au (10 nm/40 nm) were deposited by electron beam evaporation. Finally, an atomic force microscope (AFM) was used to characterize the thickness of InSe and the electrical properties were tested by Keithley 4200 in an atmospheric environment. Raman measurements were carried out using a confocal Raman microscope with a 100× objective and a Si detector. The measurements were done using a 532 nm excitation laser source in an ambient environment at room temperature. The laser power was maintained under 1 mW to avoid any local heating.

3. Results and Discussion

In this paper, we used exfoliated InSe as the channel of FETs and the variation optical contrast in microscope images of InSe flakes transferred on HfO2/Si substrate are shown in Figure 1a. As the MoS2 flakes prepared on SiO2/Si substrate [19], InSe films, prepared on HfO2/Si substrate, have different kinds of colors reflecting under the optical microscope, which can be related to nanometric changes in the thickness of films. Atomic force microscopy (AFM) results of Figure 1b show that the InSe flake is 42 nm thick with a color of light green, indicating that can be univocally identified with the color contrast areas observed in the optical image. Then, the Raman spectra and PL (Photoluminescence) spectra were both implemented with 532 nm excitation laser source at room temperature. As shown in Figure 1c, three peaks come from vibration modes of A11g, E12g, and A21g were obviously observed at 117.7 cm−1, 179.3 cm−1, and 229.1 cm−1, respectively. Other 21 vibrational modes are forbidden by Raman selected rules, relatively weak or degenerated [20]. With the extension of preservation time, no drift occurred in Raman peaks, indicating that the vibration mode is not affected by external factors. As shown in Figure 1d, peaks of PL spectra shift from 1.25 to 1.28 eV, demonstrating that the InSe flake is getting thinner, corresponding to the previous study showing that InSe changes from direct to indirect band gap material as the decrease of thickness [21]. The slight shift in PL peaks of 0.03 eV suggests a few layers decrease, which may be due to the highly oxidized properties of InSe film in air environment.
Schematic diagram and image under an optical microscope of the fabricated device are shown in Figure 2a,b. The asymmetric output curves described in Figure 2c suggested that the contact resistance is asymmetric, which is attribute to the non-ideal interface between metal and 2D InSe. The fabrication process could have a great impact on contact quality such as photo resist organic residues [22], and material damage caused by high-energy metal deposition processes [23]. Figure 2d shows the Id-Vg transport characteristics of the device at Vd = 1 V. As the Vg changed from −2 V to 2 V with a step of 0.05 mV, ID increased from 10−12 A to 10−7 A, showing the typical behavior of n-type semiconductor. With the change of gate voltage sweep direction, the current hysteresis appears, which indicates that there are many impurities and defects on the surface of 2D InSe-channel and charge traps are formed. The processes of charge and release in charge traps are responsible for the discoincidence of transfer characteristic curves when scanning direction changes. Besides, InSe is easily oxidized and sensitive to the processes of solution treatment. As a result, the maximum Ion is only 2.8 × 10−7 A, far from achieving the desired performance for InSe FET [24].
To investigate the degradation of 2D InSe FET, the devices are preserved in ambient for 1 day, 2 days, and 5 days, respectively. The corresponding transfer characteristic is shown in Figure 3a. As the preservation time extended, Ion decreases from 7.8 × 10−6 A to 2 × 10−7 A. It is due to the increase of defects on the channel surface formed by the adsorbed impurities and oxidations, causing most of the current to scatter. Vth shifts from −1.2 V to −0.2 V, suggesting that traps are formed on the channel surface. These results demonstrate that the preservation in ambient would bring drastic recession to device performance. After capping with h-BN, shown in Figure 3b, Ion decreased from 3 × 10−6 A to 7.6 × 10−7 A and Vth shifted 0.1 V. The decay degree of the device is greatly reduced. Comparing the hysteresis of InSe FET with and without h-BN, it is obvious that the passivated FET has a smaller hysteresis window. After capping by h-BN, impurities on the channel surface are reduced. In Figure 3c, changing curves of subthreshold swing (SS) of InSe FET with and without h-BN are depicted. Cap-layer of h-BN can effectively decrease SS and degradation speed of SS. The rate of decline in mobility manifests the same inference, as shown in Figure 3d. These results manifest that the degradation of 2D InSe FET can be reduced by h-BN cap-layer, which is mainly due to the reduced absorption of impurities and air molecules. However, the already occurred oxidation is irreversible, and it is responsible for the degradation after passivation by h-BN.
In order to obtain a better surface of 2D InSe FET channel, another device fabrication method is applied that we use copper hard shadow mask to define S/D contact area after InSe flakes are transferred on substrate, and then metal electrodes (Ti/Au = 10 nm/40 nm) are formed by e-beam evaporation. By using a non-photolithograph process, organic residues in contact interface are avoided and the exposure to air environment is reduced to minimize the oxidation of InSe. As a result, a high-performance InSe FET is achieved, whose output and transfer characteristic curves are described in Figure 4a,b. The nearly linear output characteristic curves demonstrate that a nearly ohmic contact is realized. According to Figure 4b, a high on/off ratio of 1.25 × 108 is achieved with a maximum Ion of 1.98 × 10−4 A at Vd = 1 V. The extracted ΔVth in linear coordinates is less than 0.1 V at Vd = 0.2, 0.5, and 1 V, indicating that an ideal channel surface is formed for this device. In addition, this device can achieve a record low SS of 70.4 mV/dec, as we know. Finally, a benchmark of SS and Ion/Ioff is depicted to compare the performance of field effect transistors fabricated using InSe and MoS2 [10,16,17,24,25,26,27,28]. According to Figure 4c, our work demonstrates the lowest SS closing to the theoretical limits of 60 mV/dec while maintaining a relative high on/off ratio. In addition, our work not only shows a significant performance improvement in similar studies of InSe FET, but is comparable to the results of high-performance MoS2 FET.

4. Conclusions

In this work, we investigate the degradation of InSe film and InSe FET in ambient. The results of Raman, PL spectra, and electronic properties demonstrate that InSe film is easy to absorb impurities and be oxidized in ambient so that the device performance has a drastic decline. With a hard shadow mask, the device can achieve high performance with on/off ratio of 1.25 × 108 and Ion of 1.98 × 10−4 A. Meanwhile, a record low SS of 70.4 mV/dec and hysteresis of 0.1 V is achieved, as we know. Our results demonstrate the huge potential of 2D InSe FET for high-performance logic devices and digital integrated circuits.

Author Contributions

Conceptualization, Y.Z. and Z.W.; methodology, X.S., H.Y., K.L., J.Y.; validation, H.Y.; formal analysis, Y.Z. and K.J.; investigation, Y.Z., X.S. and K.J.; resources, X.S., K.L. and J.Y.; writing—original draft preparation, Y.Z.; writing—review and editing, Z.W.; supervision, K.J.; project administration, Z.W.; funding acquisition, Z.W. All authors have read and agreed to the published version of the manuscript.

Funding

This work was funded by the NSFC (Grant No. 61774168, 12174423) and this work was supported by the Opening Project of Key Laboratory of Microelectronic Devices & Integrated Technology, Institute of Microelectronics, Chinese Academy of Sciences.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Tamalampudi, S.; Lu, Y.-Y.; U, R.K.; Sankar, R.; Liao, C.-D.; B, K.M.; Cheng, C.-H.; Chou, F.-C.; Chen, Y.-T. High Performance and Bendable Few-Layered InSe Photodetectors with Broad Spectral Response. Nano Lett. 2014, 14, 2800–2806. [Google Scholar] [CrossRef] [PubMed]
  2. Feng, W.; Zhou, X.; Tian, W.Q.; Zheng, W.; Hu, P. Performance improvement of multilayer InSe transistors with optimized metal contacts. Phys. Chem. Chem. Phys. 2015, 17, 3653–3658. [Google Scholar] [CrossRef] [PubMed]
  3. Sachid, A.B.; Tosun, M.; Desai, S.B.; Hsu, C.-Y.; Lien, D.-H.; Madhvapathy, S.R.; Chen, Y.-Z.; Hettick, M.; Kang, J.S.; Zeng, Y.; et al. Monolithic 3D CMOS Using Layered Semiconductors. Adv. Mater. 2016, 28, 2547–2554. [Google Scholar] [CrossRef] [PubMed]
  4. Wang, Z.; Wu, Z.; Li, X. Electronic and optical properties of monolayer InSe quantum dots. Semicond. Sci. Technol. 2021, 36, 095038. [Google Scholar] [CrossRef]
  5. Yang, H.; Xiao, M.; Cui, Y.; Pan, L.; Zhao, K.; Wei, Z. Nonvolatile memristor based on heterostructure of 2D room-temperature ferroelectric α-In2Se3 and WSe2. Sci. China Inf. Sci. 2019, 62, 220404. [Google Scholar] [CrossRef] [Green Version]
  6. Radamson, H.H.; Zhu, H.; Wu, Z.; He, X.; Lin, H.; Liu, J.; Xiang, J.; Kong, Z.; Xiong, W.; Li, J.; et al. State of the Art and Future Perspectives in Advanced CMOS Technology. Nanomaterials 2020, 10, 1555. [Google Scholar] [CrossRef]
  7. Bhuwalka, K.K.; Wu, Z.; Noh, H.-K.; Lee, W.; Cantoro, M.; Heo, Y.-C.; Jin, S.; Choi, W.; Kwon, U.; Maeda, S.; et al. In0.53Ga0.47As-Based nMOSFET Design for Low Standby Power Applications. IEEE Trans. Electron. Devices 2015, 62, 2816–2823. [Google Scholar] [CrossRef]
  8. Yao, J.; Yin, H.; Wang, W.; Li, J.; Luo, K.; Yu, J.; Zhang, Q.; Hou, Z.; Gu, J.; Yang, W.; et al. Physical Insights on Quantum Confinement and Carrier Mobility in Si, Si0.45Ge0.55, Ge Gate-All-Around NSFET for 5 nm Technology Node. IEEE J. Electron. Devices Soc. 2018, 6, 841–848. [Google Scholar] [CrossRef]
  9. Liu, L.; Kong, L.; Li, Q.; He, C.; Ren, L.; Tao, Q.; Yang, X.; Lin, J.; Zhao, B.; Li, Z.; et al. Transferred van der Waals metal electrodes for sub-1-nm MoS2 vertical transistors. Nat. Electron. 2021, 4, 342–347. [Google Scholar] [CrossRef]
  10. Arutchelvan, G.; Smets, Q.; Verreck, D.; Ahmed, Z.; Gaur, A.; Sutar, S.; Jussot, J.; Groven, B.; Heyns, M.; Lin, D.; et al. Impact of device scaling on the electrical properties of MoS2 field-effect transistors. Sci. Rep. 2021, 11, 1–11. [Google Scholar] [CrossRef]
  11. Li, M.; Yang, F.; Hsiao, Y.; Lin, C.; Wu, H.; Yang, S.; Li, H.; Lien, C.-H.; Ho, C.-H.; Liu, H.; et al. Low-Voltage Operational, Low-Power Consuming, and High Sensitive Tactile Switch Based on 2D Layered InSe Tribotronics. Adv. Funct. Mater. 2019, 29, 1809119. [Google Scholar] [CrossRef]
  12. Luo, K.; Yang, W.; Pan, Y.; Yin, H.; Zhao, C.; Wu, Z. Ab-Initio Simulations of Monolayer InSe and MoS2 Strain Effect: From Electron Mobility to Photoelectric Effect. J. Electron. Mater. 2020, 49, 559–565. [Google Scholar] [CrossRef]
  13. Sucharitakul, S.; Goble, N.J.; Kumar, U.R.; Sankar, R.; Bogorad, Z.A.; Chou, F.C.; Gao, X.P. Intrinsic Electron Mobility Exceeding 10(3) cm(2)/(V s) in Multilayer InSe FETs. Nano Lett. 2015, 15, 3815–3819. [Google Scholar] [CrossRef] [Green Version]
  14. Li, M.; Lin, C.-Y.; Yang, S.-H.; Chang, Y.-M.; Chang, J.-K.; Yang, F.-S.; Zhong, C.; Jian, W.-B.; Lien, C.-H.; Ho, C.-H.; et al. High Mobilities in Layered InSe Transistors with Indium-Encapsulation-Induced Surface Charge Doping. Adv. Mater. 2018, 30, e1803690. [Google Scholar] [CrossRef]
  15. Arora, H.; Jung, Y.; Venanzi, T.; Watanabe, K.; Taniguchi, T.; Hübner, R.; Schneider, H.; Helm, M.; Hone, J.C.; Erbe, A. Effective Hexagonal Boron Nitride Passivation of Few-Layered InSe and GaSe to Enhance Their Electronic and Optical Properties. ACS Appl. Mater. Interfaces 2019, 11, 43480–43487. [Google Scholar] [CrossRef]
  16. Wang, Y.; Zhang, J.; Liang, G.; Shi, Y.; Zhang, Y.; Kudrynskyi, Z.; Kovalyuk, Z.D.; Patanè, A.; Xin, Q.; Song, A. Schottky-barrier thin-film transistors based on HfO2-capped InSe. Appl. Phys. Lett. 2019, 115, 033502. [Google Scholar] [CrossRef] [Green Version]
  17. Ho, P.-H.; Chang, Y.-R.; Chun-Wei, C.; Li, M.-K.; Tsai, C.-A.; Wang, W.-H.; Ho, C.-H.; Chen, C.-W.; Chiu, P.-W. High-Mobility InSe Transistors: The Role of Surface Oxides. ACS Nano 2017, 11, 7362–7370. [Google Scholar] [CrossRef]
  18. Pan, Y.; Jia, K.; Huang, K.; Wu, Z.; Bai, G.; Yu, J.; Zhang, Z.; Zhang, Q.; Yin, H.; Zhang, Q. Near-ideal subthreshold swing MoS2 back-gate transistors with an optimized ultrathin HfO2 dielectric layer. Nanotechnology 2018, 30, 095202. [Google Scholar] [CrossRef]
  19. Li, H.; Zhang, Q.; Yap, C.C.R.; Tay, B.K.; Edwin, T.H.T.; Olivier, A.; Baillargeat, D. From Bulk to Monolayer MoS2: Evolution of Raman Scattering. Adv. Funct. Mater. 2012, 22, 1385–1390. [Google Scholar] [CrossRef]
  20. Lei, S.; Ge, L.; Najmaei, S.; George, A.; Kappera, R.; Lou, J.; Chhowalla, M.; Yamaguchi, H.; Gupta, G.; Vajtai, R.; et al. Evolution of the Electronic Band Structure and Efficient Photo-Detection in Atomic Layers of InSe. ACS Nano 2014, 8, 1263–1272. [Google Scholar] [CrossRef]
  21. Mudd, G.W.; Svatek, S.A.; Ren, T.; Patanè, A.; Makarovsky, O.; Eaves, L.; Beton, P.H.; Kovalyuk, Z.D.; Lashkarev, G.V.; Kudrynskyi, Z.R.; et al. Tuning the Bandgap of Exfoliated InSe Nanosheets by Quantum Confinement. Adv. Mater. 2013, 25, 5714–5718. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  22. Zhang, Y.; Jia, K.; Liu, J.; Pan, Y.; Luo, K.; Yu, J.; Zhang, Y.; Tian, H.; Wu, Z.; Yin, H. The optimization of contact interface between metal/MoS2 FETs by oxygen plasma treatment. J. Mater. Sci. Mater. Electron. 2020, 31, 9660–9665. [Google Scholar] [CrossRef]
  23. Liu, Y.; Guo, J.; Zhu, E.; Liao, L.; Lee, S.-J.; Ding, M.; Shakir, I.; Gambin, V.; Huang, Y.; Duan, X. Approaching the Schottky–Mott limit in van der Waals metal–semiconductor junctions. Nat. Cell Biol. 2018, 557, 696–700. [Google Scholar] [CrossRef] [PubMed]
  24. Tsai, T.-H.; Yang, F.-S.; Ho, P.-H.; Liang, Z.-Y.; Lien, C.-H.; Ho, C.-H.; Lin, Y.-F.; Chiu, P.-W. High-Mobility InSe Transistors: The Nature of Charge Transport. ACS Appl. Mater. Interfaces 2019, 11, 35969–35976. [Google Scholar] [CrossRef]
  25. Wu, L.; Shi, J.; Zhou, Z.; Yan, J.; Wang, A.; Bian, C.; Ma, J.; Ma, R.; Liu, H.; Chen, J.; et al. InSe/hBN/graphite heterostructure for high-performance 2D electronics and flexible electronics. Nano Res. 2020, 13, 1127–1132. [Google Scholar] [CrossRef]
  26. Jiang, J.; Li, J.; Li, Y.; Duan, J.; Li, L.; Tian, Y.; Zong, Z.; Zheng, H.; Feng, X.; Li, Q.; et al. Stable InSe transistors with high-field effect mobility for reliable nerve signal sensing. NPJ 2D Mater. Appl. 2019, 3. [Google Scholar] [CrossRef] [Green Version]
  27. Pan, Y.; Li, J.; Wang, W.; Ye, T.; Yin, H.; Huang, K.; Zhang, Z.; Zhang, Q.; Jia, K.; Wu, Z.; et al. Novel 10-nm Gate Length MoS2 Transistor Fabricated on Si Fin Substrate. IEEE J. Electron. Devices Soc. 2019, 7, 483–488. [Google Scholar] [CrossRef]
  28. Li, T.; Guo, W.; Ma, L.; Li, W.; Yu, Z.; Han, Z.; Gao, S.; Liu, L.; Fan, D.; Wang, Z.; et al. Epitaxial growth of wafer-scale molybdenum disulfide semiconductor single crystals on sapphire. Nat. Nanotechnol. 2021, 16, 1201–1207. [Google Scholar] [CrossRef]
Figure 1. (a) Photo image of exfoliated InSe flake on substrate of HfO2/Si and the thickness is tested in the dash line area. (b) AFM result of thickness along AA’ and the thickness is 42 nm, corresponding to the green InSe flakes. (c,d) The Raman and PL spectra of 42 nm InSe flake preserved for 1 day, 2 days, 3 days, 4 days, and 5 days, respectively.
Figure 1. (a) Photo image of exfoliated InSe flake on substrate of HfO2/Si and the thickness is tested in the dash line area. (b) AFM result of thickness along AA’ and the thickness is 42 nm, corresponding to the green InSe flakes. (c,d) The Raman and PL spectra of 42 nm InSe flake preserved for 1 day, 2 days, 3 days, 4 days, and 5 days, respectively.
Nanomaterials 11 03311 g001
Figure 2. (a) Schematic diagram of bottom-gated InSe FET. (b) Optical microscope image of a typical InSe FET. (c,d) Transfer and output transport characteristic curves of InSe FET. Output curves are obtained at Vg = −2 V to Vg = 2 V, with a step of 1 V, and transfer curves are measured at Vd = 1 V. The solid and dash arrows represent Vg scans from −2 V to 2 V and from 2 V to −2 V.
Figure 2. (a) Schematic diagram of bottom-gated InSe FET. (b) Optical microscope image of a typical InSe FET. (c,d) Transfer and output transport characteristic curves of InSe FET. Output curves are obtained at Vg = −2 V to Vg = 2 V, with a step of 1 V, and transfer curves are measured at Vd = 1 V. The solid and dash arrows represent Vg scans from −2 V to 2 V and from 2 V to −2 V.
Nanomaterials 11 03311 g002
Figure 3. (a) Deterioration of electrical properties of 2D InSe FET with preservation time. (b) Deterioration of electrical properties after capped with h-BN. The dash lines represent the transfer curves of Vg scanning from 2 to −2 V. Different arrows indicate the direction of scanning. (c) Recession trend of SS for devices with and without h-BN. (d) Change curve of device Δμ.
Figure 3. (a) Deterioration of electrical properties of 2D InSe FET with preservation time. (b) Deterioration of electrical properties after capped with h-BN. The dash lines represent the transfer curves of Vg scanning from 2 to −2 V. Different arrows indicate the direction of scanning. (c) Recession trend of SS for devices with and without h-BN. (d) Change curve of device Δμ.
Nanomaterials 11 03311 g003
Figure 4. Output characteristic curves (a) and transfer characteristic curves (b) of non-lithographed device. The solid and dotted lines represent voltage scanning from −2 to 2 V and from 2 to −2 V, respectively. (c) Benchmark of SS and on/off ratio of transistors in different studies, including research on InSe and MoS2.
Figure 4. Output characteristic curves (a) and transfer characteristic curves (b) of non-lithographed device. The solid and dotted lines represent voltage scanning from −2 to 2 V and from 2 to −2 V, respectively. (c) Benchmark of SS and on/off ratio of transistors in different studies, including research on InSe and MoS2.
Nanomaterials 11 03311 g004
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zhang, Y.; Sun, X.; Jia, K.; Yin, H.; Luo, K.; Yu, J.; Wu, Z. Enhancement of InSe Field-Effect-Transistor Performance against Degradation of InSe Film in Air Environment. Nanomaterials 2021, 11, 3311. https://doi.org/10.3390/nano11123311

AMA Style

Zhang Y, Sun X, Jia K, Yin H, Luo K, Yu J, Wu Z. Enhancement of InSe Field-Effect-Transistor Performance against Degradation of InSe Film in Air Environment. Nanomaterials. 2021; 11(12):3311. https://doi.org/10.3390/nano11123311

Chicago/Turabian Style

Zhang, Yadong, Xiaoting Sun, Kunpeng Jia, Huaxiang Yin, Kun Luo, Jiahan Yu, and Zhenhua Wu. 2021. "Enhancement of InSe Field-Effect-Transistor Performance against Degradation of InSe Film in Air Environment" Nanomaterials 11, no. 12: 3311. https://doi.org/10.3390/nano11123311

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop