Article

Coupled Investigation of Contact Potential and Microstructure Evolution of Ultra-Thin AlOx for Crystalline Si Passivation

1
School of Physical Science and Technology, Ningbo University, Ningbo 315211, China
2
Ningbo Institute of Materials Technology and Engineering, Chinese Academy of Sciences, Ningbo 315201, China
3
National Laboratory of Solid State Microstructures, School of Electronics Science and Engineering/Collaborative Innovation Center of Advanced Microstructures, Nanjing University, Nanjing 210093, China
4
Laboratory of Physics of Interfaces and Thin Films, CNRS, Ecole Polytechnique, Institut Polytechnique de Paris, 91128 Palaiseau, France
*
Author to whom correspondence should be addressed.
Nanomaterials 2021, 11(7), 1803; https://doi.org/10.3390/nano11071803
Submission received: 5 June 2021 / Revised: 2 July 2021 / Accepted: 8 July 2021 / Published: 12 July 2021

Abstract

:
In this work, we report the same trends for the contact potential difference measured by Kelvin probe force microscopy and the effective carrier lifetime on crystalline silicon (c-Si) wafers passivated by AlOx layers of different thicknesses and submitted to annealing under various conditions. The changes in contact potential difference values and in the effective carrier lifetimes of the wafers are discussed in view of structural changes of the c-Si/SiO2/AlOx interface thanks to high resolution transmission electron microscopy. Indeed, we observed the presence of a crystalline silicon oxide interfacial layer in as-deposited (200 °C) AlOx, and a phase transformation from crystalline to amorphous silicon oxide when they were annealed in vacuum at 300 °C.

1. Introduction

Dielectrics are widely applied for the passivation of crystalline Si (c-Si) wafers used in c-Si solar cells because they can provide both chemical and field effect passivation. Due to the parasitic shunt formed in the case of an inverted surface [1], dielectrics with negative fixed charge (Qf), such as Aluminum oxide (AlOx), are favorable to p-type c-Si, while dielectrics having a positive Qf, such as amorphous hydrogenated silicon nitride (a-SiNx:H), are better suited to n-type material. Different techniques have been developed to grow AlOx layers: (i) sputtering, which requires an extrinsic hydrogenation step to obtain a good passivation [2]; (ii) atomic layer deposition (ALD) [3,4,5,6,7]; (iii) oxidation of Al with the help of other oxide materials, such as TiO2 [8]; (iv) inline plasma-enhanced chemical vapor deposition [9], etc. Among these techniques, ALD can provide extremely good passivation quality. The advantage of ALD is its precise control of the thickness at atomic level with perfect uniformity and conformality. Two main types of ALD have been developed including plasma-enhanced ALD (PEALD) and thermal ALD. By taking advantage of the negative fixed charge density of AlOx itself, a passivation with surface recombination velocity (SRV) close to 10 cm/s has been achieved for p-type silicon [10]. Two main approaches have been developed to improve the passivation quality provided by AlOx including thermal annealing [11,12,13,14] and light-soaking [15,16,17].
The passivation quality mainly depends on the interfacial states or defects between the c-Si substrate and the AlOx layer. Therefore, studying the c-Si/AlOx interface is an important issue. For example, investigation of the interfacial composition with the help of transmission electron microscopy (TEM) has revealed the existence of a mixed SiOx layer [18,19,20]. A high Qf density, as measured by corona charging experiments, provides a very strong field effect passivation [21]. Second harmonic generation (SHG) measurements have indicated a thickness independent negative Qf suggesting that the charge must be located at the SiOx/AlOx interface [22], which results from the local reconstruction of the interfacial SiOx layer after annealing in Ar ambient at 525 °C for 15 min [23]. Such changes can affect the work function of the material, which depends on its doping level and the presence of surface dipoles and surface states, which can be measured by Kelvin probe [24,25]. Therefore, AlOx, layers have been widely studied by Kelvin probe. To cite a few examples: (i) the determination of the surface potential uniformity of AlOx [26], (ii) imaging of the charge in AlOx gate oxides [27], (iii) estimation of the total charge density in metal/AlOx/SiO2/Si structures [28], and (iv) study of the surface potential difference between AlOx-coated graphene and AlOx-coated Cu [29]. In this work, we used thermal ALD to deposit AlOx layers. To investigate the properties of AlOx under different conditions including as-deposited state and after thermal treatments, the contact potential difference (CPD) of AlOx layers was measured with the help of Kelvin probe force microscopy (KPFM). High resolution TEM (HRTEM) was used to characterize the evolution of the microstructure of AlOx layers under different thermal treatments.

2. Experimental Procedure

AlOx layers with three different thicknesses (1.5 nm, 5 nm and 10 nm) were deposited using thermal ALD technique (Savannah Ultratech, Cambridge, UK). The thickness of AlOx is controlled by the number of cycles. Double side polished Si wafers (FZ, (100) n-type, 4-inch diameter, 250 μm, 1–10 Ω·cm) were used as substrates for a symmetrical deposition. The same deposition temperature of 200 °C was used for all AlOx passivation layers. The detailed ALD deposition conditions are presented in Table 1. In order to remove the native oxide, the c-Si wafers were dipped into HF (5%) for 30 s prior to AlOx deposition. KPFM (Asylum research, Oxford instruments, Buckinghamshire, UK) was used to investigate the AlOx passivated samples. Conductive atomic force microscopy (AFM) tips (AC240TM from Olympus, Tokyo, Japan) were used, which have a doped Si cantilever and a Pt coating. The wavelength in the KPFM system is 850 nm. The laser spot size is around 3 × 9 µm, which is smaller than the cantilever. Moreover, the laser spot is well positioned away from the cantilever edge to minimize the parasitic illumination from AFM laser. The KPFM measurements in this work were performed under humidity below 30%, since Sugimura et al. report that low humidity can allow a good potential contrast [30]. The measurements were performed with a planar configuration of the sample since the ultra-thin thickness of AlOx layers will cause interpretation difficulties when investigated in cross-section configuration. A diamond pen was used to scratch the sample surface in order to create a sharp interface between AlOx and the c-Si substrate. Afterwards, an ultrasonic treatment of samples in deionized water was applied for 60 min in order to remove the scratch-produced Si flakes, since too much surface roughness can cause measurement artifacts, difficulty of data interpretation and breaking of tips.
TEM analyses of different AlOx deposited layers required a lamella preparation. Thus, cross-section lamellas were prepared using a standard lift-out procedure within a Focus Ion Beam dual beam microscope (FIB, FEI-Scios DualBeam, Thermo Fisher Scientific, Waltham, MA, USA). Transmission Electron Microscopy (TEM) analyses were performed on 2 different Titan Themis transmission electron microscopes operating at 300 kV and 200 kV accelerating voltage. For the TEM observation, we used the low dose mode of the electron microscope and a 4k/4k direct detection electron (DDE) camera. The DDE camera is a very sensitive camera which uses very low dose (max 25 e2) for the image acquisition. In our case, the max dose used with the TEM operating at 300 kV was 10 e2. For the chemical analyses we used a Titan-Themis operating at 200 kV equipped with a Cs probe corrector and a SuperX detector that allows chemical analyses of light and heavy elements with a spatial resolution within picometer range. The experimental conditions were set so that the total current within the probe used for the chemical analysis was about 85 pA. As elements of interest, we chose silicon with Kα = 1.74 keV ionization edge, oxygen with Kα = 0.523 keV, and aluminum with Kα = 1.48 keV ionization edge. Carbon and platinum protective layers were deposited on AlOx layer prior to the FIB milling process in order to prevent the Ga ion implantation during the milling process.

3. Results and Discussion

The effective minority carrier lifetime of our samples was measured by quasi steady-state photoconductance (QSSPC, Sinton Instruments, Boulder, CO, USA). The results are presented in Figure 1, where AlOx passivation layers with three different thicknesses (1.5 nm, 5 nm and 10 nm) are shown. Three states of the samples were characterized, including as-deposited, annealed in air and annealed in vacuum (0.1 Pa), separately. The annealing temperature and annealing time are kept the same for all these treatments at 300 °C for 15 min. Note that the effective carrier lifetime was recorded at the injection level of 1015 cm−3. The corresponding lifetime values are summarized in Figure 1d. The as-deposited sample with 1.5 nm AlOx has a lifetime of 17 µs and it decreases to 12 µs after annealing in air. Its value increases to 31 µs after annealing in vacuum. For 5 nm AlOx passivated sample (Figure 1b), the as-deposited lifetime (200 µs) increases to 233 µs but decreases to 132 µs when annealed in air and vacuum, respectively. For 10 nm of AlOx, their lifetime value increases from 152 µs to 272 µs then reaches 777 µs once the as-deposited sample experiences annealing in air and annealing in vacuum, respectively. A conclusion can be made that AlOx passivation with different layer thicknesses exhibits different trends even if they were submitted to the same thermal annealing, indicating that the layer properties and their evolution depend on AlOx layer thickness.
In order to investigate the influence of thermal treatment on passivation quality of AlOx layers, AFM and KPFM were used, where AFM provides information on the morphology and KPFM provides CPD values. The corresponding AFM and KPFM mappings of c-Si/AlOx samples are presented in Table 2. The diamond-introduced scratching channel can be clearly observed with some bumps at the scratching edge. A clean c-Si surface without the flakes has been obtained thanks to the ultrasonic treatment.
In order to have quantitative information from AFM and KPFM, a profile across the scratching channel between AlOx and c-Si substrate is made, marked as red lines in Table 2. Note that both AFM and KPFM profiles were collected from the same position for the same sample. The contact potential difference (CPD) between the tip and sample surface can be defined as follows:
C P D = φ t φ s e
where, φ t and φ s are the work function of the conductive AFM tip and sample, respectively, and e is the elementary charge. The corresponding CPD profiles are presented in Figure 2. The CPD corresponding to the edge of the flat zone (marked as the solid line) can be defined as the CPD of c-Si/AlOx layer stacks. The CPD of c-Si substrate surface is defined as the value of the first turning point of the CPD curve, which is marked by the black dotted line. The CPD difference Δ CPD between AlOx and c-Si can be considered as the absolute CPD of interfacial layer, which can be defined as follows:
| Δ   C P D | = φ A l O x φ S i
The CPD values can be measured as 0.233 V (0.5 V), 0. 375 V (0. 189 V), and 0.183 V (0.340 V) for 1.5, 5 and 10 nm AlOx in the as-deposited state presented by white columns (annealed in vacuum presented by grey columns), respectively, as summarized in Figure 2g. Therefore, we can observe that the CPD of c-Si/AlOx for 1.5 and 10 nm sample increases after annealing in vacuum, while it decreases for 5 nm AlOx. Based on Equation (2), we can calculate that the work function of a given layer increases with the increase of its Δ CPD. Then, we can infer that, for 1.5 and 10 nm AlOx, the work function of c-Si/AlOx increases, while for 5 nm, it decreases. Comparing with the corresponding minority carrier lifetimes in Figure 1d, we can conclude that the changes in the work function follow the same trends as the effective minority carrier lifetime.
To understand the work function evolution for AlOx layers, TEM was used to study their microstructure under different thermal treatments. The characterization results are shown in Figure 3. A HRTEM image of as-deposited 1.5 nm AlOx layer is shown in Figure 3a with a zoom of interface shown in Figure 3b, where a partially crystallized amorphous SiOx (a-SiOx) phase can be observed. The inset of Figure 3b shows the corresponding Fourier transform. The inter plane distance can be calculated to be 1.64 Å. The low magnification and HRTEM images for 5 nm AlOx are presented in Figure 3c,d, respectively. Inset of Figure 3d shows the corresponding HRTEM image, where the interfacial SiOx layer reveals again a crystalline structure with inter plane distance of 1.6 Å. The oxidation of Si substrate could be due to the interfacial oxygen diffusion during AlOx deposition. The chemical distribution of different elements of the SiOx layer is also studied by scanning transmission electron microscopy-high angle annular dark-field (STEM-HAADF) and energy dispersive X-ray (EDX) spectroscopy. The STEM-HAADF image is shown in Figure 3e. A closer analysis of STEM-EDX mapping allowed the identification of the multilayer structure as shown in Figure 3d, with the clear crystalline SiOx (c-SiOx) layer at the interface between the c-Si wafer and AlOx. The total crystallization of interfacial SiOx occurs during longer deposition time (thicker AlOx layer). Surprisingly, when the AlOx layer is annealed in vacuum, the amorphization of the c-SiOx layer occurs as shown in Figure 3g,h, which correspond to low and high magnification of TEM, respectively, with its HRTEM image shown in the inset.
The evolution of the surface passivation provided by the AlOx layers submitted to different annealing conditions can be discussed based on the presence of hydrogen in AlOx layers [31,32]. The difference in ambient conditions can affect the diffusion of hydrogen, which can be more important for the sample annealed in vacuum compared to that of the sample annealed in air. Concerning the 1.5 nm AlOx passivation layer, in the case of annealing in air, the SiOx layer turns out to be more crystallized, probably due to exothermic reactions of H confined at the interface. In the case of 5 nm AlOx passivation, when annealed in air, a relatively thicker AlOx layer could effectively prevent hydrogen atoms from escaping, and eventually keep them at the c-Si/AlOx interface to form a hydrogen-saturated chemical passivation. However, when annealing in vacuum, the hydrogen in the passivation layer can be pumped away; hence, it cannot effectively saturate the dangling bonds. Therefore, the passivation quality after annealing in vacuum is even lower than that of the as-deposited sample because of dehydroxylation at the AlOx layer. As compared to 5 nm AlOx passivation, more Al-OH bonds are formed during the deposition of the 10 nm AlOx layer. Thus, the thicker AlOx layer can prevent the dehydroxylation even when annealed in vacuum. When it is annealed in air, a slightly better passivation quality can be obtained because of the inhibition of dehydroxylation due to the ambient air conditions. However, when the sample is annealed in vacuum, dehydroxylation occurs more easily. As a consequence, more H atoms can be released from Al-OH bonds. Therefore, a better passivation quality can be obtained when 10 nm AlOx layer is annealed in vacuum.
From the above HRTEM results, we can conclude that for the sample annealed in vacuum, the SiOx interfacial layer exhibits an amorphous structure, while its thickness is maintained at the same value as for the as-deposited state. It has been reported that a thin amorphous AlOx is more stable than a crystalline one due to the surface and interface defects [33]. Therefore, one can expect that the amorphous state of the interfacial SiOx is favored as compared to its crystalline state when annealed at 300 °C for 15 min. The decrease of the work function upon annealing for the 1.5 nm AlOx layer contrasts with the 5 and 10 nm AlOx layers and can be discussed as follows. The work function values for c-Si and a-Si are 4.85 eV and 4.66 eV, respectively. Accordingly, we suggest a tendency that the work function of SiOx decreased from crystalline to amorphous. Therefore, a higher work function of c-SiOx is expected as compared to a-SiOx. Based on the HRTEM images in Figure 3d,h, the interfacial SiOx changed from crystalline to amorphous state after annealing; therefore, the corresponding work function decreases. Literature reported that in a nonzero net charge sample including Qf, a higher work function can be achieved compared to zero net charge sample [34]. Therefore, we can assume that AlOx with higher work function has larger Qf. For 1.5 and 10 nm AlOx, their work functions increase after annealing in vacuum resulting from an increase of Qf and, therefore, leading to an improvement of the passivation quality. On the contrary, a decrease of work function due to a lower Qf will cause a degradation of the passivation quality in the case of 5 nm AlOx. This is consistent with minority carrier lifetime results as presented in Figure 1.

4. Conclusions

In summary, the influence of thermal treatments on AlOx with three thicknesses (1.5 nm, 5 nm and 10 nm) was investigated by KPFM and HRTEM. We have found that AlOx passivation with different layer thicknesses exhibits different trends even if they were exposed to the same thermal annealing. The passivation quality increases when AlOx was annealed in vacuum for 1.5 and 10 nm, while it decreases for the 5 nm sample. From KPFM measurements of samples after annealing in vacuum, an increase of work function is observed in the case of 1.5 and 10 nm AlOx layers, while a decrease of work function is obtained for the 5 nm AlOx layer, which has been related to the amorphization of the interfacial crystalline SiOx layer as evidenced by HRTEM.

Author Contributions

Conceptualization, Z.Z. and W.C.; investigation, Z.Z., Y.Z. and I.F.; writing—original draft preparation, W.C. and Z.Z.; writing—review and editing, Z.Z., J.A., R.G., Y.Z., J.Y., L.Y., I.F., P.R.i.C. and W.C.; supervision, W.C.; project administration, W.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are contained within the article.

Acknowledgments

FIB lamella preparation and STEM-HAADF EDX characterizations have been performed in the frame of the French Government program of investment for the future (Programme d’Investissement d’Avenir—TEMPOS Equipex—ANR-10-EQPX-50, pole NanoTEM) and ANR-IEED-002-01. Part of the TEM analyses were performed at CIMEX—Centre interdisciplinaire de microscopie électronique de l’X, which is gratefully acknowledge for the use of the electron microscopes at École Polytechnique.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Vermang, B.; Cornagliotti, E.; Prajapati, V.; John, J.; Poortmans, J.; Mertens, R. Assessment of the illumination dependency of Al2O3 and SiO2 rear-passivated p-type silicon solar cells. Phys. Status Solidi RRL Rapid Res. Lett. 2012, 6, 259–261. [Google Scholar] [CrossRef]
  2. Zhang, X.; Cuevas, A. Plasma hydrogenated, reactively sputtered aluminium oxide for silicon surface passivation. Phys. Status Solidi RRL Rapid Res. Lett. 2013, 7, 619–622. [Google Scholar] [CrossRef]
  3. Repo, P.; Talvitie, H.; Li, S.; Skarp, J.; Savin, H. Silicon Surface Passivation by Al2O3: Effect of ALD Reactants. Energy Procedia 2011, 8, 681–687. [Google Scholar] [CrossRef] [Green Version]
  4. Kotipalli, R.; Delamare, R.; Poncelet, O.; Tang, X.; Francis, L.A.; Flandre, D. Passivation effects of atomic-layer-deposited aluminum oxide. EPJ Photovolt. 2013, 4, 45107. [Google Scholar] [CrossRef]
  5. Töfflinger, J.A.; Laades, A.; Korte, L.; Leendertz, C.; Montañez, L.M.; Stürzebecher, U.; Sperlich, H.-P.; Rech, B. PECVD-AlOx/SiNx passivation stacks on wet chemically oxidized silicon: Constant voltage stress investigations of charge dynamics and interface defect states. Sol. Energy Mater. Sol. Cells 2015, 135, 49–56. [Google Scholar] [CrossRef]
  6. Lee, Y.S.; Gershon, T.; Todorov, T.K.; Wang, W.; Winkler, M.T.; Hopstaken, M.; Gunawan, O.; Kim, J. Atomic Layer Deposited Aluminum Oxide for Interface Passivation of Cu2ZnSn(S,Se)4 Thin-Film Solar Cells. Adv. Energy Mater. 2016, 6, 1600198. [Google Scholar] [CrossRef]
  7. Dingemans, G.; Kessels, W.M.M. Status and prospects of Al2O3-based surface passivation schemes for silicon solar cells. J. Vac. Sci. Technol. A 2012, 30, 040802. [Google Scholar] [CrossRef] [Green Version]
  8. Yang, X.; Bi, Q.; Ali, H.; Davis, K.; Schoenfeld, W.V.; Weber, K. High-Performance TiO2-Based Electron-Selective Contacts for Crystalline Silicon Solar Cells. Adv. Mater. 2016, 28, 5891–5897. [Google Scholar] [CrossRef]
  9. Töfflinger, J.A.; Laades, A.; Leendertz, C.; Montañez, L.M.; Korte, L.; Stürzebecher, U.; Sperlich, H.-P.; Rech, B. PECVD-AlOx/SiNx Passivation Stacks on Silicon: Effective Charge Dynamics and Interface Defect State Spectroscopy. Energy Procedia 2014, 55, 845–854. [Google Scholar] [CrossRef] [Green Version]
  10. Hoex, B.; Schmidt, J.; Bock, R.; Altermatt, P.P.; van de Sanden, M.C.M.; Kessels, W.M.M. Excellent passivation of highly doped p-type Si surfaces by the negative-charge-dielectric Al2O3. Appl. Phys. Lett. 2007, 91, 112107. [Google Scholar] [CrossRef] [Green Version]
  11. Zhao, Y.; Zhou, C.; Zhang, X.; Zhang, P.; Dou, Y.; Wang, W.; Cao, X.; Wang, B.; Tang, Y.; Zhou, S. Passivation mechanism of thermal atomic layer-deposited Al2O3 films on silicon at different annealing temperatures. Nanoscale Res. Lett. 2013, 8, 114. [Google Scholar] [CrossRef] [Green Version]
  12. Pawlik, M.; Vilcot, J.P.; Halbwax, M.; Aureau, D.; Etcheberry, A.; Slaoui, A.; Schutz-Kuchly, T.; Cabal, R. Electrical and Chemical Studies on Al2O3 Passivation Activation Process. Energy Procedia 2014, 60, 85–89. [Google Scholar] [CrossRef] [Green Version]
  13. Kühnhold-Pospischil, S.; Saint-Cast, P.; Richter, A.; Hofmann, M. Activation energy of negative fixed charges in thermal ALD Al2O3. Appl. Phys. Lett. 2016, 109, 061602. [Google Scholar] [CrossRef]
  14. Lebreton, F.; Zauner, A.; Bulkin, P.; Silva, F.; Filonovich, S.; Cabarrocas, P.R. Benefits of a thermal drift during atomic layer deposition of Al2O3 for C-Si passivation. In Proceedings of the 2017 IEEE 44th Photovoltaic Specialist Conference (PVSC), Washington, DC, USA, 25–30 June 2017; pp. 1237–1240. [Google Scholar]
  15. Xie, M.; Yu, X.; Qiu, X.; Yang, D. Light-soaking enhanced passivation of Al2O3 on crystalline silicon surface. Solar Energy Mater. Sol. Cells 2019, 191, 350–355. [Google Scholar] [CrossRef]
  16. Heikkinen, I.T.S.; Koutsourakis, G.; Virtanen, S.; Yli-Koski, M.; Wood, S.; Vähänissi, V.; Salmi, E.; Castro, F.A.; Savin, H. AlOx surface passivation of black silicon by spatial ALD: Stability under light soaking and damp heat exposure. J. Vac. Sci. Technol. A 2020, 38, 022401. [Google Scholar] [CrossRef]
  17. Desthieux, A.; Sreng, M.; Bulkin, P.; Florea, I.; Drahi, E.; Bazer-Bachi, B.; Vanel, J.-C.; Silva, F.; Posada, J.; Cabarrocas, P.R. Detection of stable positive fixed charges in AlOx activated during annealing with in situ modulated PhotoLuminescence. Solar Energy Mater. Sol. Cells 2021, 230, 111172. [Google Scholar] [CrossRef]
  18. Liao, B.; Stangl, R.; Ma, F.; Mueller, T.; Lin, F.; Aberle, A.G.; Bhatia, C.S.; Hoex, B. Excellentc-Si surface passivation by thermal atomic layer deposited aluminum oxide after industrial firing activation. J. Phys. D Appl. Phys. 2013, 46, 385102. [Google Scholar] [CrossRef]
  19. Hsu, C.-H.; Cho, Y.-S.; Wu, W.-Y.; Lien, S.-Y.; Zhang, X.-Y.; Zhu, W.-Z.; Zhang, S.; Chen, S.-Y. Enhanced Si Passivation and PERC Solar Cell Efficiency by Atomic Layer Deposited Aluminum Oxide with Two-step Post Annealing. Nanoscale Res. Lett. 2019, 14, 139. [Google Scholar] [CrossRef] [PubMed]
  20. Noircler, G.; Lebreton, F.; Drahi, E.; de Coux, P.; Warot-Fonrose, B. STEM-EELS investigation of c-Si/a-AlOx interface for solar cell applications. Micron 2021, 145, 103032. [Google Scholar] [CrossRef]
  21. Hoex, B.; Schmidt, J.; van de Sanden, M.C.M.; Kessels, W.M.M. Crystalline silicon surface passivation by the negative-charge-dielectric Al2O3. In Proceedings of the 2008 IEEE 33rd Photovoltaic Specialists Conference, San Diego, CA, USA, 11–16 May 2008; pp. 1–4. [Google Scholar]
  22. Terlinden, N.M.; Dingemans, G.; van de Sanden, M.C.M.; Kessels, W.M.M. Role of field-effect on c-Si surface passivation by ultrathin (2–20 nm) atomic layer deposited Al2O3. Appl. Phys. Lett. 2010, 96, 112101. [Google Scholar] [CrossRef] [Green Version]
  23. Dou, Y.N.; He, Y.; Huang, C.Y.; Zhou, C.L.; Ma, X.G.; Chen, R.; Chu, J.H. Role of surface fixed charge in the surface passivation of thermal atomic layer deposited Al2O3 on crystalline-Si. Appl. Phys. A 2012, 109, 673–677. [Google Scholar] [CrossRef]
  24. Melitz, W.; Shen, J.; Kummel, A.C.; Lee, S. Kelvin probe force microscopy and its application. Surf. Sci. Rep. 2011, 66, 1–27. [Google Scholar] [CrossRef]
  25. Garrillo, P.A.F.; Grévin, B.; Chevalier, N.; Borowik, Ł. Calibrated work function mapping by Kelvin probe force microscopy. Rev. Sci. Instrum. 2018, 89, 043702. [Google Scholar] [CrossRef] [PubMed]
  26. Zhang, J.; Hultqvist, A.; Zhang, T.; Jiang, L.; Ruan, C.; Yang, L.; Cheng, Y.; Edoff, M.; Johansson, E.M.J. Al2O3 Underlayer Prepared by Atomic Layer Deposition for Efficient Perovskite Solar Cells. ChemSusChem 2017, 10, 3810–3817. [Google Scholar] [CrossRef] [Green Version]
  27. Ludeke, R. Electrical characterization of gate oxides by scanning probe microscopies. J. Non Cryst. Solids 2002, 303, 150–161. [Google Scholar] [CrossRef]
  28. Khosla, R.; Rolseth, E.G.; Kumar, P.; Vadakupudhupalayam, S.S.; Sharma, S.K.; Schulze, J. Charge Trapping Analysis of Metal/Al2O3/SiO2/Si, Gate Stack for Emerging Embedded Memories. IEEE Trans. Device Mater. Reliab. 2017, 17, 80–89. [Google Scholar] [CrossRef]
  29. Collins, L.; Kilpatrick, J.I.; Weber, S.A.L.; Tselev, A.; Vlassiouk, I.V.; Ivanov, I.N.; Jesse, S.; Kalinin, S.V.; Rodriguez, B.J. Open loop Kelvin probe force microscopy with single and multi-frequency excitation. Nanotechnology 2013, 24, 475702. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  30. Sugimura, H.; Ishida, Y.; Hayashi, K.; Takai, O.; Nakagiri, N. Potential shielding by the surface water layer in Kelvin probe force microscopy. Appl. Phys. Lett. 2002, 80, 1459–1461. [Google Scholar] [CrossRef]
  31. Guerra-Nuñez, C.; Döbeli, M.; Michler, J.; Utke, I. Reaction and Growth Mechanisms in Al2O3 deposited via Atomic Layer Deposition: Elucidating the Hydrogen Source. Chem. Mater. 2017, 29, 8690–8703. [Google Scholar] [CrossRef]
  32. Dingemans, G.; Einsele, F.; Beyer, W.; van de Sanden, M.C.M.; Kessels, W.M.M. Influence of annealing and Al2O3 properties on the hydrogen-induced passivation of the Si/SiO2 interface. J. Appl. Phys. 2012, 111, 093713. [Google Scholar] [CrossRef] [Green Version]
  33. Jeurgens, L.P.H.; Sloof, W.G.; Tichelaar, F.D.; Mittemeijer, E.J. Thermodynamic stability of amorphous oxide films on metals: Application to aluminum oxide films on aluminum substrates. Phys. Rev. B 2000, 62, 4707–4719. [Google Scholar] [CrossRef] [Green Version]
  34. Polak, L.; Wijngaarden, R.J. Two competing interpretations of Kelvin probe force microscopy on semiconductors put to test. Phys. Rev. B 2016, 93, 195320. [Google Scholar] [CrossRef] [Green Version]
Figure 1. Minority carrier lifetime as a function of the minority carrier density for symmetrical deposition of AlOx with three different thicknesses: (a) 1.5 nm, (b) 5 nm, (c) 10 nm. (d) Summary of effective carrier lifetime upon different thermal treatments.
Figure 1. Minority carrier lifetime as a function of the minority carrier density for symmetrical deposition of AlOx with three different thicknesses: (a) 1.5 nm, (b) 5 nm, (c) 10 nm. (d) Summary of effective carrier lifetime upon different thermal treatments.
Nanomaterials 11 01803 g001
Figure 2. KPFM characterization of six different AlOx passivation samples after annealing in vacuum (right side) as compared to their as-deposited state (left side). (a,b) 1.5 nm AlOx. (c,d) 5 nm AlOx. (e,f) 10 nm AlOx. (g) Summary of |Δ CPD| values for 1.5, 5 and 10 nm AlOx.
Figure 2. KPFM characterization of six different AlOx passivation samples after annealing in vacuum (right side) as compared to their as-deposited state (left side). (a,b) 1.5 nm AlOx. (c,d) 5 nm AlOx. (e,f) 10 nm AlOx. (g) Summary of |Δ CPD| values for 1.5, 5 and 10 nm AlOx.
Nanomaterials 11 01803 g002
Figure 3. (a) HRTEM image of as-deposited 1.5 nm AlOx layer, with the enlarged view in (b). Inset showing the Fourier transform. (c) Low magnification TEM image of as-deposited 5 nm AlOx layer with HRTEM image shown in (d). (e) STEM-HAADF image of as-deposited 5 nm AlOx layer. (f) STEM-HAADF EDX mapping of as-deposited 5 nm AlOx layer. (g) Low magnification TEM image of 5 nm AlOx layer annealed in vacuum and the corresponding HRTEM image in (h). Insets of the figure (b,d,h) show the corresponding HRTEM images, evidencing the crystalline/amorphous character of different layers. Red dashed lines are provided as a guide to the eye for different layers.
Figure 3. (a) HRTEM image of as-deposited 1.5 nm AlOx layer, with the enlarged view in (b). Inset showing the Fourier transform. (c) Low magnification TEM image of as-deposited 5 nm AlOx layer with HRTEM image shown in (d). (e) STEM-HAADF image of as-deposited 5 nm AlOx layer. (f) STEM-HAADF EDX mapping of as-deposited 5 nm AlOx layer. (g) Low magnification TEM image of 5 nm AlOx layer annealed in vacuum and the corresponding HRTEM image in (h). Insets of the figure (b,d,h) show the corresponding HRTEM images, evidencing the crystalline/amorphous character of different layers. Red dashed lines are provided as a guide to the eye for different layers.
Nanomaterials 11 01803 g003
Table 1. ALD cycle used in the work. Deposition chamber is flushed by 20 SCCM of N2. (SCCM: standard cubic centimeters per minute).
Table 1. ALD cycle used in the work. Deposition chamber is flushed by 20 SCCM of N2. (SCCM: standard cubic centimeters per minute).
TMAPurgeH2OPurge
Time (s)0.01530.0153
Table 2. AFM (morphology) and KPFM (CPD) mapping of six AlOx samples: as-deposited and annealed in vacuum for three different AlOx thicknesses.
Table 2. AFM (morphology) and KPFM (CPD) mapping of six AlOx samples: as-deposited and annealed in vacuum for three different AlOx thicknesses.
SamplesAs-DepositedAnnealed in Vacuum
MorphologyCPDMorphologyCPD
1.5 nm Nanomaterials 11 01803 i001 Nanomaterials 11 01803 i002 Nanomaterials 11 01803 i003 Nanomaterials 11 01803 i004
5 nm Nanomaterials 11 01803 i005 Nanomaterials 11 01803 i006 Nanomaterials 11 01803 i007 Nanomaterials 11 01803 i008
10 nm Nanomaterials 11 01803 i009 Nanomaterials 11 01803 i010 Nanomaterials 11 01803 i011 Nanomaterials 11 01803 i012
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zheng, Z.; An, J.; Gong, R.; Zeng, Y.; Ye, J.; Yu, L.; Florea, I.; Roca i Cabarrocas, P.; Chen, W. Coupled Investigation of Contact Potential and Microstructure Evolution of Ultra-Thin AlOx for Crystalline Si Passivation. Nanomaterials 2021, 11, 1803. https://doi.org/10.3390/nano11071803

AMA Style

Zheng Z, An J, Gong R, Zeng Y, Ye J, Yu L, Florea I, Roca i Cabarrocas P, Chen W. Coupled Investigation of Contact Potential and Microstructure Evolution of Ultra-Thin AlOx for Crystalline Si Passivation. Nanomaterials. 2021; 11(7):1803. https://doi.org/10.3390/nano11071803

Chicago/Turabian Style

Zheng, Zhen, Junyang An, Ruiling Gong, Yuheng Zeng, Jichun Ye, Linwei Yu, Ileana Florea, Pere Roca i Cabarrocas, and Wanghua Chen. 2021. "Coupled Investigation of Contact Potential and Microstructure Evolution of Ultra-Thin AlOx for Crystalline Si Passivation" Nanomaterials 11, no. 7: 1803. https://doi.org/10.3390/nano11071803

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop